电子束蒸发SiO2薄膜的棱台凹坑模型及其验证

,  ,  ,  ,  ,  ,  ,  ,  , 

上一篇

下一篇

秦文斌, 张富荣, 宗华, 孙潇莹, 周飞, 张海斌, 严凯, 荣皓, 宿非凡, 邓辉. 电子束蒸发SiO2薄膜的棱台凹坑模型及其验证[J]. 真空科学与技术学报, 2026, 46(9): 893-900. doi: 10.13922/j.cnki.cjvst.202604025
引用本文: 秦文斌, 张富荣, 宗华, 孙潇莹, 周飞, 张海斌, 严凯, 荣皓, 宿非凡, 邓辉. 电子束蒸发SiO2薄膜的棱台凹坑模型及其验证[J]. 真空科学与技术学报, 2026, 46(9): 893-900. doi: 10.13922/j.cnki.cjvst.202604025
Wenbin QIN, Furong ZHANG, Hua ZONG, Xiaoying SUN, Fei ZHOU, Haibin ZHANG, Kai YAN, Hao RONG, Feifan SU, Hui DENG. Frustum Pit Model of Electron Beam Evaporated SiO2 Thin Films and Its Experimental Verification[J]. zkkxyjsxb, 2026, 46(9): 893-900. doi: 10.13922/j.cnki.cjvst.202604025
Citation: Wenbin QIN, Furong ZHANG, Hua ZONG, Xiaoying SUN, Fei ZHOU, Haibin ZHANG, Kai YAN, Hao RONG, Feifan SU, Hui DENG. Frustum Pit Model of Electron Beam Evaporated SiO2 Thin Films and Its Experimental Verification[J]. zkkxyjsxb, 2026, 46(9): 893-900. doi: 10.13922/j.cnki.cjvst.202604025

电子束蒸发SiO2薄膜的棱台凹坑模型及其验证

    通讯作者: E-mail: sufeifan@ustc.edu.cn;  huid@ustc.edu.cn
  • 中图分类号: TB43

Frustum Pit Model of Electron Beam Evaporated SiO2 Thin Films and Its Experimental Verification

    Corresponding authors: Feifan SU, sufeifan@ustc.edu.cn ;  Hui DENG, huid@ustc.edu.cn
  • MSC: TB43

  • 摘要: SiO2薄膜在半导体和超导电子学领域应用广泛。针对电子束蒸发SiO2中“挖坑效应”导致的薄膜均匀性持续劣化问题,本文通过实验证实传统“小圆锥体模型”在长效沉积(>15 min)中预测边缘与中心膜厚比误差超过8.80%,指出其失效核心在于忽略了坑形的动态演化对厚度分布的影响。针对此问题,本文基于热扩散机理与线扫描工艺的实际棱台坑形特征,构建了棱台凹坑动态演化模型,进而确立了坑壁倾角与时间的定量函数关系,并引入修正因子补偿有效蒸发面积的动态扩展效应。结果显示,棱台模型对第4点的预测误差小于0.20%,较原模型精度提升约90%。研究揭示了热扩散是主导坑形演化的核心物理机制,该模型为量子处理器电子束蒸发工艺优化、均匀性预测、工艺窗口设计与精准控制提供了理论依据和量化工具。
  • 加载中
  • 图 1  小圆锥体蒸发模型[17]

    Figure 1.  Small cone evaporation model[17]

    图 2  电子束蒸发镀膜装置示意图

    Figure 2.  Schematic diagram of electron beam evaporation system

    图 3  不同沉积时间的SiO2薄膜样品。(a)7 min,(b)10 min,(c)17 min

    Figure 3.  Physical images of SiO2 thin film samples with different deposition times. (a) 7 min, (b) 10 min, (c) 17 min

    图 4  电子束蒸发SiO2棱台凹坑实物图

    Figure 4.  Physical image of SiO2 frustum pit model fabricated by EBE

    图 5  棱台凹坑蒸发模型示意图。(a)三维立体图,(b)截面图,(c)俯视图

    Figure 5.  Schematic diagram of frustum pit evaporation model. (a) 3D stereogram, (b) cross-section view, (c) top view

    图 6  角度$ \theta ( {^\circ} ) $、修正因子$ f(t) $和膜厚比分别随时间$ t $ (min)变化的趋势图。(a)角度和与时间变化关系,(b)棱台模型修正因子与时间的关系,(c)不同模型厚度比与时间的关系

    Figure 6.  Trend plots of angle and film thickness ratio vs. time, respectively. (a) relationship between angles and time variation, (b) relationship between the frustum pit model correction factor and time, (c) relationship between different model thickness ratios and time

    表 1  不同沉积时间下SiO2薄膜的膜厚数据

    Table 1.  Film thickness data of SiO2 thin films at different deposition times

    时间/min实验$ \theta $
    /(°)
    中心膜厚/nm中间膜厚/nm边缘膜厚/nm边缘与中心
    厚度比值/%
    763.44102.99102.94102.3099.33%
    1059.98116.84116.44115.6498.98%
    1750.56198.24197.53196.0798.90%
    下载: 导出CSV

    表 2  小圆锥模型计算结果与实验结果对比

    Table 2.  Comparison between small cone model theoretical calculation and experimental results

    时间t/min实测厚度比/%$ g(t) $锥/%绝对误差/%
    799.3393.675.66
    1098.9892.456.53
    1798.9090.108.80
    下载: 导出CSV

    表 3  模型计算结果与实验结果对比

    Table 3.  Comparison between theoretical calculation and experimental results

    t/mincotθ棱θ棱台/(°)实测厚度比/%$ g(t) $锥/%$ f(t) $$ G(t) $棱/%
    70.49563.6099.3393.671.0699.27
    100.60158.9798.9892.451.0799.00
    170.80751.0298.9090.101.1098.85
    220.93546.9598.5088.631.11预98.38预
    下载: 导出CSV
  • [1] Deus C, von Ardenne GmbH. Large-area high-rate electron beam evaporation: the PVD process of choice for demanding future applications[J]. Vakuum in Forschung und Praxis, 2023, 35(S1): 66−68
    [2] Mencia R, Lin Y H, Manucharyan V. Superconducting titanium nitride films grown by directional reactive evaporation[J]. Journal of Applied Physics, 2021, 130(22): 225109 doi: 10.1063/5.0048819
    [3] 袁世豪, 徐均琪, 苏俊宏, 等. 高损伤阈值激光薄膜的制备方法[J]. 应用光学, 2023, 44(6): 1185−1194 (in Chinese) doi: 10.5768/JAO202344.0610004 Yuan S H, Xu J Q, Su J H, et al. Review of preparation methods of laser films with high damage threshold[J]. Journal of Applied Optics, 2023, 44(6): 1185−1194 doi: 10.5768/JAO202344.0610004
    [4] 张以忱. 真空镀膜技术与设备(第二版)[M]. 北京: 冶金工业出版社, 2021: 1−10 (in Chinese) Zhang Y C. (2nd edition)[M]. Beijing: Metallurgical Industry Press, 2021: 1−10
    [5] Kim S H, Lee M Y, Woo K, et al. A study on thin film uniformity in a roll-to-roll thermal evaporation system for flexible OLED applications[J]. International Journal of Precision Engineering and Manufacturing, 2017, 18(8): 1111−1117 doi: 10.1007/s12541-017-0130-4
    [6] Schweizer P M. Film thickness and film thickness uniformity[M]//Schweizer P M. Premetered coating methods: attractiveness and limitations. Cham: Springer, 2022: 387−452
    [7] 郭俊寒, 季鸿雨, 于海洋, 等. 电子束蒸发Cu膜的厚度均匀性和准确性的研究[J]. 仪器与设备, 2024, 12(4): 527−534 (in Chinese) doi: 10.12677/iae.2024.124069 Guo J H, Ji H Y, Yu H Y, et al. Study on thickness uniformity and accuracy of electron beam evaporation Cu thin film[J]. Instrumentation and Equipments, 2024, 12(4): 527−534 doi: 10.12677/iae.2024.124069
    [8] 谭深. 镀膜机蒸发源位形对膜厚均匀性的影响[J]. 真空科学与技术, 1985, 5(2): 39−43 (in Chinese) Tan S. Influence of the location and the form of evaporation source on the uniformity of film thickness in the film-plating mechine[J]. Vacuum Science and Technology (China), 1985, 5(2): 39−43
    [9] Holland L, Steckelmacher W. The distribution of thin films condensed on surfaces by the vacuum evaporation method[J]. Vacuum, 1952, 2(4): 346−364 doi: 10.1016/0042-207X(52)93784-6
    [10] 王宁, 魏朝阳, 邵建达, 等. 电子束自动扫描SiO2材料沉积速率控制实验研究[J]. 中国激光, 2010, 37(10): 2615−2619 (in Chinese) doi: 10.3788/CJL20103710.2615 Wang N, Wei C Y, Shao J D, et al. Experimentation of deposition rate control of SiO2 by E-beam auto-sweeping[J]. Chinese Journal of Lasers, 2010, 37(10): 2615−2619 doi: 10.3788/CJL20103710.2615
    [11] 潘永刚, 刘政, 王奔, 等. 电子束蒸发球面夹具系统膜厚均匀性的研究[J]. 激光与光电子学进展, 2021, 58(5): 0523001 (in Chinese) doi: 10.3788/LOP202158.0523001 Pan Y G, Liu Z, Wang B, et al. Research on film thickness uniformity of electron beam evaporation spherical fixture system[J]. Laser & Optoelectronics Progress, 2021, 58(5): 0523001 doi: 10.3788/LOP202158.0523001
    [12] 夏志林, 赵元安, 黄才华, 等. 基于平板夹具的电子束蒸发沉积薄膜中的挖坑效应分析[J]. 真空, 2008, 45(6): 12−16 (in Chinese) Xia Z L, Zhao Y A, Huang C H, et al. Discussion on digging effect on thin flims deposited by electron beam evaporation with substrate held by plate jig[J]. Vacuum, 2008, 45(6): 12−16
    [13] 夏志林, 薛亦渝, 郭培涛, 等. 挖坑效应对球形夹具下电子束蒸发沉积薄膜厚度均匀性的影响[J]. 材料导报, 2009, 23(14): 15−18 (in Chinese) doi: 10.3321/j.issn:1005-023X.2009.14.005 Xia Z L, Xue Y Y, Guo P T, et al. Influence of digging effect on films thickness uniformity for electron beam evaporating onto sphere jig[J]. Materials Review, 2009, 23(14): 15−18 doi: 10.3321/j.issn:1005-023X.2009.14.005
    [14] Guo C, Kong M D. Fabrication of ultralow stress TiO2/SiO2 optical coatings by plasma ion-assisted deposition[J]. Coatings, 2020, 10(8): 720 doi: 10.3390/coatings10080720
    [15] Gudmundsson J T, Anders A, von Keudell A. Foundations of physical vapor deposition with plasma assistance[J]. Plasma Sources Science and Technology, 2022, 31(8): 083001 doi: 10.1088/1361-6595/ac7f53
    [16] Wen S T, Zhao F, Li Y L, et al. Modeling of heat transfer in target material during the electron beam evaporation process[J]. Vacuum, 2024, 222: 112972 doi: 10.1016/j.vacuum.2024.112972
    [17] 付学成, 张洪波, 权雪玲, 等. 电子束蒸发挖坑效应膜厚均匀性的计算新方法[J]. 实验室研究与探索, 2018, 37(3): 30−32,41 (in Chinese) doi: 10.3969/j.issn.1006-7167.2018.03.009 Fu X C, Zhang H B, Quan X L, et al. A new calculating method for digging effect on thickness uniformity of films[J]. Research and Exploration in Laboratory, 2018, 37(3): 30−32,41 doi: 10.3969/j.issn.1006-7167.2018.03.009
    [18] Rastgou M, Hülagü D, Danilenko A, et al. Comparison of thin-film thickness measurements using ellipsometry and reflectometry with uniform samples[J]. Metrologia, 2026, 63(1): 015006 doi: 10.1088/1681-7575/ae3964
    [19] Baynes P C, Nagarajan T. Evaporation characteristics of electron beam gun heated sources[J]. Active and Passive Electronic Components, 1984, 11(2): 697139
    [20] Dikshit B, Zende G R, Bhatia M S, et al. Convection in molten pool created by a concentrated energy flux on a solid metal target[J]. Physics of Fluids, 2009, 21(8): 084105 doi: 10.1063/1.3210763
    [21] Carslaw H S, Jaeger J C. Conduction of heat in solids[M]. Oxford: Oxford University Press, 1959
    [22] Paek U C, Gagliano F P. Thermal analysis of laser drilling processes[J]. IEEE Journal of Quantum Electronics, 1971, 7(6): 277 doi: 10.1109/jqe.1971.1076653
    [23] Harrach R J. Analytical solutions for laser heating and burnthrough of opaque solid slabs[J]. Journal of Applied Physics, 1977, 48(6): 2370−2383 doi: 10.1063/1.323999
    [24] 森西優, 前田祐作. 単一反射スペクトルのみでの金属薄膜の膜厚・光学定数推定モデルの開発[J]. 電気学会論文誌E(センサ・マイクロマシン部門誌), 2025, 145(10): 220−225 (in Japanese) doi: 10.1541/ieejsmas.145.220 Morinishi Y, Maeda Y. Development of the model for estimating thickness and optical constants of metallic thin films using only reflection spectrum[J]. IEEJ Transactions on Sensors and Micromachines, 2025, 145(10): 220−225 doi: 10.1541/ieejsmas.145.220
    [25] Sun Y H, Wang C Y, Liu C Y, et al. An optimization framework for infrared interferometric inversion of epitaxial layer parameters based on Fresnel reflection and least squares method[C]//Proceedings of SPIE 13994, Second International Conference on Information Optics and Optoelectronics Technology, Kunming: SPIE, 2025: 139940L
    [26] Willmott C J, Matsuura K. Advantages of the mean absolute error (MAE) over the root mean square error (RMSE) in assessing average model performance[J]. Climate Research, 2005, 30: 79−82 doi: 10.3354/cr030079
  • 加载中
图( 6) 表( 3)
计量
  • 文章访问数:  84
  • HTML全文浏览数:  84
  • PDF下载数:  1
  • 施引文献:  0
出版历程
  • 收稿日期:  2026-04-29
  • 刊出日期:  2026-09-30

电子束蒸发SiO2薄膜的棱台凹坑模型及其验证

    通讯作者: E-mail: sufeifan@ustc.edu.cn; 
    通讯作者: huid@ustc.edu.cn
  • 1. 济南量子技术研究院 济南 250101
  • 2. 合肥国家实验室量子计算部 合肥 230094
  • 3. 中国科学技术大学量子信息与量子科技创新研究院 合肥 230026

摘要: SiO2薄膜在半导体和超导电子学领域应用广泛。针对电子束蒸发SiO2中“挖坑效应”导致的薄膜均匀性持续劣化问题,本文通过实验证实传统“小圆锥体模型”在长效沉积(>15 min)中预测边缘与中心膜厚比误差超过8.80%,指出其失效核心在于忽略了坑形的动态演化对厚度分布的影响。针对此问题,本文基于热扩散机理与线扫描工艺的实际棱台坑形特征,构建了棱台凹坑动态演化模型,进而确立了坑壁倾角与时间的定量函数关系,并引入修正因子补偿有效蒸发面积的动态扩展效应。结果显示,棱台模型对第4点的预测误差小于0.20%,较原模型精度提升约90%。研究揭示了热扩散是主导坑形演化的核心物理机制,该模型为量子处理器电子束蒸发工艺优化、均匀性预测、工艺窗口设计与精准控制提供了理论依据和量化工具。

English Abstract

  • 电子束蒸发镀膜技术是现代薄膜制备的重要技术手段之一,广泛应用于半导体和超导电子学器件制造等领域[1-4]。在电子束蒸发过程中,高能电子束轰击蒸发源材料,使其受热蒸发并在衬底表面沉积形成薄膜。膜厚均匀性是评价薄膜质量的关键指标,其直接影响薄膜的性能、应力和翘曲情况,从而影响器件良率[5, 6]。

    由于蒸发源材料热物理性质存在差异性,电子束蒸发过程一般呈现两种不同的蒸发源形貌。对导热性良好的金属材料,蒸发时材料熔融呈半球形,可近似为理想点源或小平面源蒸发,能够形成均匀性较好的薄膜[7];与导热性良好的金属材料不同,SiO2作为典型的高熔点、低热导率介质材料,在电子束轰击下,蒸发源中心区域与边缘存在剧烈的温度梯度,导致材料以升华方式直接气化逐渐形成凹陷坑洞,即所谓的"挖坑"效应[7]。挖坑效应的形成涉及热传导、材料相变及质量输运等复杂过程。

    挖坑效应会显著改变蒸发源的空间发射特性[7],导致薄膜厚度均匀性随着沉积时间增加而逐步恶化,影响单一膜层以及对应器件性能和良率水平。电子束蒸发镀膜中薄膜厚度均匀性的研究已系统涵盖蒸发源理论建模、几何与工艺参数影响、挖坑效应机理及夹具系统优化等关键维度[8-16]。付学成等[17]提出了小圆锥体蒸发模型计算挖坑效应对膜厚均匀性的影响。现有的小圆锥体模型基于静态形貌假设,忽略了坑形随时间的动态演化,存在一定的局限性,其在长效工艺中的边缘膜厚与中心膜厚比预测精度仍有待检验。

    本文旨在通过实验验证发现原小圆锥体模型的局限性,然后结合实际凹坑几何形貌分析偏差产生的机理,进而基于热扩散机制构建更符合物理规律的棱台凹坑动态演化模型。新模型建立了坑壁倾角与时间的定量函数以及晶圆边缘膜厚与中心膜厚比的数学公式;最后通过独立实验验证了模型在外推预测中的可靠性。

    • 付学成等[17]提出了一种改进的小圆锥体蒸发模型。如图1所示,该模型认为在电子束蒸发SiO2过程中,束斑位置从源材料表面逐渐向下移动,形成一个小圆锥体或类小圆锥体的坑。整个过程可看作蒸发源材料按照小圆锥体顶角方向向外均匀扩散分布在顶角为$ 2\theta $、半径为$ R $的部分球体内。

      在衬底上任意点$ M $薄膜的厚度,可看作过$ M $点垂直平面$ {m}_{2} $,交球冠表面$ {M}_{2} $和圆锥$ {M}_{1} $两点之间的高度之和,设$ l $为$ M $点距离衬底中心$ O $点的距离。可得边缘与中心膜厚比$ g(t) $:

      式中$ T $为边缘点膜厚,$ {T}_{0} $为中心点膜厚,$ R $为球冠半径,$ l $为测量点到中心$ O $点的距离,$ \theta $为圆锥半顶角。

    • 实验所用设备为Kurt J. Lesker公司生产的PVD 200型电子束蒸发镀膜设备,图2为设备示意图。设备本底真空抽至6.67×10−5 Pa,工作真空约为1.33×10−3 Pa,衬底距离蒸发源表面的高度差$ H $为65.00 cm,棱台模型测量的蒸发半径$ R $约为65.40 cm。蒸发源材料为纯度99.999%(5N)的SiO2锭,尺寸为上口直径3.5 cm,下口直径2.7 cm,高度1.7 cm,放置于容量为15 cc的石墨坩埚。电子枪工作电压为6 kV,电子束采用线扫描模式进行蒸发,聚焦于SiO2蒸发源表面的有效束斑尺寸约为28 mm × 4 mm,其中长轴沿扫描方向Y,短轴沿X方向分布,扫描频率设置为50 Hz,沉积速率设置为2 Å/s(设备自带晶振膜厚监控系统实时闭环控制沉积速率),样品台旋转速率10 rpm,分别在6英寸硅衬底上先后制备了3个不同沉积时间(7 min、10 min和17 min)的SiO2薄膜样品。

      SiO2薄膜厚度采用J.A.WOOllam M系列椭偏仪进行测试,测试模型基于柯西模型进行薄膜厚度的拟合测试[18]。为计算样品的中心与边缘的厚度比以及整片的均匀性,实验中分别测试每个样品的中心点($ l=0 $)、中间点($ l=\text{3.5 cm} $)和边缘点($ l=\text{7.5 cm} $)处SiO2薄膜的厚度,重复测量3次求取平均值,并记录。后续文中所提及的厚度比均指边缘点处平均膜厚/中心点处平均膜厚的比值。挖坑形貌通过千分尺多次测量各沉积时间点蒸发源的坑深$ h $与凹坑边长并取平均值,对应的实际角度由边长与坑深的长度计算$ \tan \theta $值后反推得到角度$ \theta $,相关测试结果见表1。通过前3个($ t=\text{7 min} $、10 min和17 min)样品的角度数据,拟合确定角度与时间的公式。

    • 基于上述实验方法,对不同沉积时间(7 min、10 min、17 min)下的SiO2薄膜进行测试与分析,结果如下,样品实物图见3所示,样品的颜色不同与膜厚差异性有关。所有样品的膜厚数据均使用椭偏仪测得,数据如表1所示。

      从表中数据分析,随着沉积时间的增加,坑壁半顶角$ \theta $逐渐减小,膜厚均匀性逐渐变差。

      将表1中$ t=\text{7 min} $,$ t=\text{10 min} $和$ t=\text{17 min} $ 时对应的角度数据,分别代入小圆锥体模型边缘与中心处厚度比公式 (1) 分别计算得到该模型预测的对应沉积时间下的厚度比,见下表2。

      随沉积时间增加,小圆锥模型的预测误差呈单调扩大趋势,最大偏差高达8.80%。这表明传统小圆锥模型未能捕捉到蒸发源形貌演化的物理本质,存在明显的局限性,导致膜厚比预测精度低。

    • 为解决传统小圆锥体模型在预测边缘与中心的膜厚比失效问题,从热量传输和相变动力学的角度进一步考虑凹坑的形成机理。在电子束蒸发工艺中,电子束的扫描方式主要分为两种,一种为点扫描,另一种为线扫描;其中金属材料,如铝一般选用点扫描模式,而介质材料如SiO2通常选择线扫描模式进行薄膜的制备,所以在实际应用场景中观察到SiO2等介质材料的凹坑形态非小圆锥体而更接近棱台结构,如图4和图5(a)所示。

      为准确描述坑壁倾角随时间的演化规律,建立时间与厚度比的关系并提高模型对厚度比预测的精度,本文根据蒸发料的实际形貌,提出了新的基本假设:

      (1)凹坑为棱台结构,$ y $方向取单位长度$ {L}_{y}=1 $。

      (2)坑底宽度 $ {w}_{0} $为常数,由电子束最小聚焦尺寸决定。

      (3)坑口宽度 $ {w}_{1} $、坑深$ h $随时间演化。

      (4)坑壁与法线面夹角为 $ \theta $。

      根据几何关系,建立沉积时间$ t $与挖坑深度$ h $演化的关系:

      由坑壁倾角 $ \theta $ 可知,坑深$ h $对应的水平投影为 $ h\tan \theta $,两侧共 2$ h\tan \theta $,

      则梯形截面宽度关系:$ {w}_{1}={w}_{0}+2 h\tan \theta $

      梯形截面积:$ A=\dfrac{1}{2}({w}_{0}+{w}_{1})h $

      面积化简将$ {w}_{1}={w}_{0}+2 h\tan \theta $代入面积公式:

      单位长度体积因取单位长度$ {L}_{y} $=1,则体积为截面积乘以长度:

      体积 $ V=A{L}_{y}={w}_{0}h+{h}^{2}\tan \theta $

      根据质量守恒定律,建立凹坑体积(坑深)与凹坑时间演化的关系:

      假设蒸发速率恒定,体积随时间线性增长:$ V=Kt $,$ K $为与材料、电子束功率相关的常数。

    • 在经典物理和材料科学中,对于一维热扩散或物质扩散,特征长度$ L $与时间$ t $的关系通常表示为$ L(t)=\sqrt{Dt} $,其中D是扩散系数。当电子束作用于极低热导率的SiO2(绝缘体)表面时,局部区域因吸收高能电子而迅速升温,根据经典传热学中半无限大物体的瞬态热传导模型[16, 19-21],热量从束斑中心向材料内部传导,导致材料发生熔化或升华界面推进,其物理演化过程受热扩散机制主导[22]。Harrach等人验证了在恒定热源作用下,绝缘体蒸发熔化深度$ h $与时间$ t $的平方根成正比[23]。基于上述理论依据,坑深$ h $随演化时间$ t $的函数关系可表述为:$ h(t)=C\sqrt{t} $,$ V={w}_{0}h+{h}^{2}\tan \theta $

      两边同时除以$ t $:

      整理得到$ \cot \theta $表达式:$ \tan \theta =\dfrac{K}{{C}^{2}}-\dfrac{{w}_{0}}{C} \cdot \dfrac{1}{\sqrt{t}} $

      令$ A=\dfrac{K}{{C}^{2}},B=-\dfrac{{w}_{0}}{C} $,则模型为:

      则角度$ \theta $与时间$ t $的通用的关系式为:

      此即坑壁角度与时间演化的关系式。

      将(3)代入到(1)式,可得到小圆锥体模型厚度比$ g(t) $与时间的关系式:

      对现有(4)式进一步分析发现,小圆锥体模型在预测膜厚比时未考虑蒸发源尺寸的随着时间的增加而在不断扩展的问题,故其厚度比模型预测值较实际值偏差较大,且随时间增加而扩大。

      因此增加可根据实验获得的修正因子$ f(t) $ 补偿有效蒸发面积扩大效应(补偿几何投影的面积),则棱台模型厚度比$ G(t) $公式:

      其中修正系数$ f(t) $包括源尺寸、遮挡等多个因素。

      电子束蒸发时,总有效蒸发面积分为坑底蒸发面积和侧壁蒸发面积,其中侧壁蒸发面积因持续受热而持续贡献蒸发通量,故有总有效蒸发面积$ {A}_{\text{总}}(t) $:

      进一步简化得到:

      且蒸发修正系数与有效蒸发面积成正相关,即$ f(t)\propto{A}_{\text{总}}(t) $ 则有:

      其中$ {k}_{1} $为蒸发源基础的贡献,与电子束线扫描最小尺寸(坑底宽度)有关,$ {k}_{2} $表征凹坑演化对有效蒸发面积的增强效应,两者均为当前工艺条件下的常数,可通过实验数据拟合得到。动态修正因子f (t)用于综合描述凹坑演化过程中有效蒸发面积变化、侧壁贡献、几何遮挡以及实际工艺条件对沉积通量的影响。

      将公式(7)代入公式(4)得到棱台模型的厚度比公式:

    • 为结合实验数据推导适用于本文实验条件的棱台模型的公式(2)和公式(9)的常数项。对表1中时间与角度的实验数据进行预处理,计算得到不同时间点$ \tan \theta $实验值;并作变量转换,令通用模型公式(2)$ \tan \theta =A+\dfrac{B}{\sqrt{t}} $ 转换成:

      其中因变量$ y:\tan \theta $

      自变量$ x $:$ \dfrac{1}{\sqrt{t}} $

      利用最小二乘法[24-25]对模型公式进行拟合,确定适用于当前工艺条件的模型公式为:

      分别使用7 min,10 min和17 min时的理论计算角度与实际测量数据,对修正因子$ f(t) $进行计算,令小圆锥模型的计算的厚度比为$ g(t) $,实际测量得到膜厚比为$ F(t) $,有: $ f(t)=\dfrac{F(t)}{g(t)} $,结果见下表3。

      利用最小二乘法,拟合求得:

      再将公式(12)代入公式(9),则棱台模型的厚度比$ G(t) $公式为:

    • 为进一步验证模型的准确性,制备了沉积时间为22 min的薄膜样品(除沉积时间外,所有工艺条件均与上文其他样品相同),以此验证模型对工艺的预测能力。将$ t\text{=22 min} $代入公式(13),计算得到棱台模型预测厚度比98.38%,与实验测量值98.50%相近,相差<0.2%,结果见上表3。

      根据实验数据和棱台模型分别计算了不同沉积时间下的角度,绘制了角度与时间的关系图;并进一步计算了实验样品实测膜厚比、棱台模型以及改良的小圆锥模型的对应的厚度比,绘制了厚度比与时间的关系图,见下图6。

      从上述各图表数据分析,由前三个样品的数据拟合确定常数项的时间与角度函数关系式与实验数据吻合极好,符合角度随着时间增加逐渐变小的现象。小圆锥模型计算得到边缘与中心膜厚的厚度比快速下降,均匀性随时间呈线性恶化趋势,但实验数据显示实际膜厚比并未随时间(或角度)快速下降,而是呈缓慢下降的趋势;同时基于小圆锥体模型计算的厚度比与实际数据的偏差随着时间增加而变化,说明该模型过于简化,只考虑了角度减小“遮挡效应”变强,导致厚度比下降,未考虑到实际蒸发源扩展对蒸发的影响。

    • 从膜厚比趋势来看,原小圆锥模型同本文的棱台模型一样,也能表征膜厚比随时间增加而降低的趋势,但小圆锥模型计算得到的边缘与中心膜厚的厚度比随时间呈快速下降的特点,均匀性则呈线性恶化趋势;这与实际膜厚比随时间(或角度)呈缓慢下降的现象冲突。SiO2属于升华型材料,其蒸发过程凹坑形貌会随沉积时间持续演化。随着凹坑深度增加,坑壁倾角逐渐变化,蒸发区域的空间几何关系随之改变,并产生一定的自遮挡效应,使大角度出射蒸汽通量受到限制。小圆锥体模型过于简化,只考虑了角度减小,“遮挡效应”变强导致厚度比下降,忽略了实际蒸发源扩展对蒸发的影响,从而影响模型计算结果。本文模型通过引入时间相关的坑壁倾角函数$ \tan \theta $和动态修正因子f (t),对上述形貌演化导致的沉积通量变化进行了等效修正。在实际沉积过程中,样品台旋转进一步降低了蒸发源非轴对称结构对膜厚分布的影响。因此,在本文实验时间范围内,该模型能够较好反映凹坑演化对膜厚均匀性的影响。

      为进一步评估模型的准确性,本文引用平均绝对误差(Mean Absolute Error,MAE)和均方根误差(Root Mean Square Error,RMSE)[26]来评估模型偏离程度,计算得到棱台模型对应的厚度比平均绝对误差和均方根误差均<0.50%,拟合优度为0.94,而小圆锥模型的平均绝对误差和均方根误差分别为7.72%和7.90%。原小圆锥模型加入时间与角度的关系后,虽然其具备了预测各时间节点膜厚比的能力,但其精度较棱台凹坑模型存在巨大差距。

      进一步分析时间$ t $与角度$ \theta $的关系公式 $ \tan \theta =\dfrac{5.77}{\sqrt{t}}-0.16 $,坑壁倾角$ \theta $的演化并非单纯由电子束的几何投影决定,而是受到热能横向扩散的强烈制约。随着时间增加,热扩散影响扩大,导致坑壁逐渐“变陡”,这与实验观测到的角度随时间减小的趋势完全一致,最终 $ \theta $趋于一个稳定值$ {\theta }_{sat} $。这与实验中观察到的“棱台凹坑”的稳定倾角现象相契合。

    • 本文遵循“实验证伪—机理分析—模型修正—盲测验证”的科学路径,通过实验证实了传统小圆锥体模型在预测长效沉积SiO2时存在边缘与中心膜厚比偏差较大的问题。基于热扩散物理机制与线扫描工艺下的实际坑形特征,构建了基于棱台凹坑动态演化的几何蒸发模型。通过理论推导,建立了沉积时间与凹坑侧壁倾角的定量函数关系 $ \tan \theta =\dfrac{5.77}{\sqrt{{t}}}-0.16 $,并结合热扩散方程阐明热扩散主导的熔池形貌演化机制是决定凹坑几何特征的关键物理过程。进一步根据实际实验引入非线性修正因子$ f(t)=0.69+0.062 \times \sqrt{t+(5.77-0.16\sqrt{t}{)}^{2}} $,补偿了原小圆锥模型对边缘沉积增强效应的忽略,显著提升了厚度分布预测精度。实验验证表明:棱台模型预测的膜厚比与实测值吻合良好,平均绝对误差(MAE)和均方根误差均小于0.5%,棱台模型具有优异的外推可靠性。本文不仅从物理层面揭示了热扩散与蒸发动力学的耦合规律,阐明了凹坑形貌演化对膜厚均匀性的调控机制,而且该显式函数可直接嵌入工艺控制系统,无需实时测量凹坑角度,为电子束蒸发工艺中沉积参数优化、膜厚均匀性精准预测及工艺窗口设计提供了理论依据与量化工具。

      基于本文后续研究可引入蒸发速率动态变化、衬底温度等其他工艺参数,完善模型适用性,并拓展至其他介质材料与复杂衬底条件;此外,对于超长时间沉积条件下遮挡效应逐步增强对模型外推精度的影响,也需进一步开展实验与理论验证,以增强模型在极端工艺条件下的可靠性。

    参考文献 (26)

目录

/

返回文章
返回