面向超高分辨微显示的金属凸点制备工艺研究

,  ,  ,  ,  ,  ,  , 

上一篇

下一篇

程龙, 张树钱, 李俊龙, 刘源, 黄杰, 刘良伟, 龙志炜, 吴朝兴. 面向超高分辨微显示的金属凸点制备工艺研究[J]. 真空科学与技术学报, 2026, 46(9): 881-892. doi: 10.13922/j.cnki.cjvst.202606015
引用本文: 程龙, 张树钱, 李俊龙, 刘源, 黄杰, 刘良伟, 龙志炜, 吴朝兴. 面向超高分辨微显示的金属凸点制备工艺研究[J]. 真空科学与技术学报, 2026, 46(9): 881-892. doi: 10.13922/j.cnki.cjvst.202606015
Long CHENG, Shuqian ZHANG, Junlong LI, Yuan LIU, Jie HUANG, Liangwei LIU, Zhiwei LONG, Chaoxing WU. Fabrication Technology of Metal Bumps for Ultra-high Resolution Micro-display[J]. zkkxyjsxb, 2026, 46(9): 881-892. doi: 10.13922/j.cnki.cjvst.202606015
Citation: Long CHENG, Shuqian ZHANG, Junlong LI, Yuan LIU, Jie HUANG, Liangwei LIU, Zhiwei LONG, Chaoxing WU. Fabrication Technology of Metal Bumps for Ultra-high Resolution Micro-display[J]. zkkxyjsxb, 2026, 46(9): 881-892. doi: 10.13922/j.cnki.cjvst.202606015

面向超高分辨微显示的金属凸点制备工艺研究

    通讯作者: E-mail: chaoxing_wu@fzu.edu.cn
  • 中图分类号: TN305.96

Fabrication Technology of Metal Bumps for Ultra-high Resolution Micro-display

    Corresponding author: Chaoxing WU, chaoxing_wu@fzu.edu.cn
  • MSC: TN305.96

  • 摘要: 超高密度微纳显示器件对互连凸点提出了极小间距、高均匀性的严苛要求。本文以电化学沉积为核心工艺,结合紫外激光直写技术制备超细间距铜(Cu)金属凸点阵列。实验优化光刻工艺以获得高分辨率微孔掩模,采用硫酸铜酸性电镀液体系进行生长,探究电流密度、沉积时间等参数对凸点形貌、高度均匀性、内部结构及界面结合性能的影响。最终实现了中心间距2 μm的超高密度凸点的高效制备,阵列尺寸达到5000 × 5000,凸点高度可达2 μm,阵列高度不均匀性低至2.92%。所得铜凸点阵列表面形貌光滑有序、无短路桥连,内部结构致密无孔洞及杂质等缺陷,去除冗余种子层后仍保持稳定结构。基于该工艺,在氮化镓发光二极管(GaN-LED)外延片上制备并成功实现了250 × 250阵列发光,验证了实现12700 PPI像素密度的可行性。本研究或将为超高分辨率微显示器件的互连键合技术与高效发光器件的研发与产业化应用提供参考。
  • 加载中
  • 图 1  金属凸点的制备流程

    Figure 1.  The fabrication process of metal bumps

    图 2  实验装置及样品形貌。(a)实验装置示意图;(b)-(e)不同阵列尺寸样品宏观形貌

    Figure 2.  Experimental setup and sample morphology. (a) Schematic diagram of the experimental setup, (b)–(e) macroscopic morphologies of samples with different array sizes

    图 3  不同曝光频率下的光刻图案及参数分析。(a)-(h)不同曝光频率下激光显微镜扫描形貌,(i)不同曝光频率下曝光剂量变化,(j)不同曝光频率下图案深度与直径,(k)不同曝光频率下图案的孔深/直径

    Figure 3.  Lithographic patterns and parameter analysis under different exposure frequencies. (a)–(h) Laser scanning microscope morphologies, (i) relationship between frequency and exposure energy, (j) pattern depth and diameter, (k) depth-to-diameter ratio

    图 4  不同沉积时间对凸点形貌的影响。(a)、(b)沉积时间为2 min时制备的样品光学显微图和SEM图;(c)、(d)沉积时间为4 min时时制备的样品光学显微图和SEM图;(e)、(f)沉积时间为6 min时制备的样品光学显微图和SEM图;(g)、(h)沉积时间为8 min时制备的样品光学显微图和SEM图;(i)、(j)沉积时间为10 min时制备的样品光学显微图和SEM图;(k)本节实验样品宏观形貌;(l)不同样品的高度不均匀性和轮廓不均匀性

    Figure 4.  Effects of different deposition times on bump morphology. (a), (b) Optical microscopy and SEM images of the sample prepared at a deposition time of 2 min; (c), (d) optical microscopy and SEM images of the sample prepared at a deposition time of 4 min; (e), (f) optical microscopy and SEM images of the sample prepared at a deposition time of 6 min; (g), (h) optical microscopy and SEM images of the sample prepared at a deposition time of 8 min; (i), (j) optical microscopy and SEM images of the sample prepared at a deposition time of 10 min; (k) macroscopic morphology of the experimental samples; (l) height non-uniformity and profile non-uniformity of different samples

    图 5  不同电流密度对凸点形貌的影响。(a)、(b)电流密度为2 mA/cm2时制备的样品光学显微图和SEM图;(c)、(d)电流密度为4 mA/cm2时制备的样品光学显微图和SEM图;(e)、(f)电流密度为6 mA/cm2时制备的样品光学显微图和SEM图;(g)、(h)电流密度为8 mA/cm2时制备的样品光学显微图和SEM图;(i)、(j)电流密度为10 mA/cm2时制备的样品光学显微图和SEM图;(k)不同样品的高度不均匀性;(l)不同样品的轮廓不均匀性

    Figure 5.  Effects of different current densities on bump morphology. (a), (b) Optical microscopy and SEM images of the sample prepared at a current density of 2 mA/cm2; (c), (d) optical microscopy and SEM images of the sample prepared at a current density of 4 mA/cm2; (e), (f) optical microscopy and SEM images of the sample prepared at a current density of 6 mA/cm2; (g), (h) optical microscopy and SEM images of the sample prepared at a current density of 8 mA/cm2; (i), (j) optical microscopy and SEM images of the sample prepared at a current density of 10 mA/cm2; (k) height non-uniformity of different samples; (l) profile non-uniformity of different samples

    图 6  种子层刻蚀原理及形貌表征。(a)ICP刻蚀种子层原理示意,(b)-(d)刻蚀前形貌,(e)-(g)刻蚀后形貌

    Figure 6.  Etching principle and morphology characterization of seed layer. (a) Schematic diagram of ICP seed layer etching principle, (b)-(d) morphologies before etching, (e)-(g) morphologies after etching

    图 7  超高密度发光器件制备流程及驱动现象。(a)-(f)器件制备流程,(g)-(i)外加驱动下的器件发光现象

    Figure 7.  Fabrication process and driving phenomena of ultra-high-density light-emitting devices. (a)-(f) Device fabrication process, (g)-(i) light-emitting phenomena of the devices under external driving

    表 1  电镀液组成

    Table 1.  Ingredients of electroplating solution

    物质成分含量主要作用
    CuSO4·5H2O220 g/L提供Cu2+
    H2SO435 g/L维持酸性,提高溶液电导率
    Cl−30 mg/L促进铜阳极均匀溶解
    PEG-6000200 mg/L抑制高电流区域沉积速率
    SPS1 mg/L促进Cu2+还原沉积
    JGB3 mg/L改善镀层平整度
    下载: 导出CSV
  • [1] Kong K, Choi H J, Han H j, et al. 1-nm-thick epitaxial AlN passivation for highly efficient flexible InGaN red micro-LEDs[J]. Nature Communications, 2025, 16(1): 5607−5607 doi: 10.1038/s41467-025-60886-z
    [2] Li Y, Guo Y, Li J, et al. Micro-LED microdisplays driven by carbon nanotube active-matrix backplanes[J]. ACS Nano, 2025, 19(25): 22837−22848 doi: 10.1021/acsnano.5c00672
    [3] Li J, Guo Y, Huang W, et al. Quantum dot micro/nano patterns: advanced manufacturing for controlled assembly[J]. International Journal of Extreme Manufacturing, 2026, 8(4): 042008−042008 doi: 10.1088/2631-7990/ae5296
    [4] Anand N, Ghosh D K, Abbes A, et al. Ultra-dense green InGaN/GaN nanoscale pixels with high luminescence stability and uniformity for near-eye displays[J]. ACS Nano, 2024, 18(39): 26882−26890 doi: 10.1021/acsnano.4c08224
    [5] Goshonoo K, Okuno K, Ohya M, et al. Demonstration of InGaN full-color monolithic micro-LED display using stacking and selective removal of the light-emitting layer[J]. Applied Physics Express, 2025, 18(2): 022003−022003 doi: 10.35848/1882-0786/adb5ec
    [6] Li J, Qiu J, Xie B, et al. Light-emitting MOS junction for ultrahigh-resolution quantum dot displays[J]. Nano Energy, 2024, 120
    [7] Li J, Guo Y, Wang K, et al. Shadow-assisted sidewall emission for achieving submicron linewidth light source by using normal UV photolithography[J]. Nano-Micro Letters, 2025, 17(10): 49−62 doi: 10.1007/s40820-025-01737-w
    [8] Li Z, Liu Y, Jiang H, et al. Vertical GaN-On-GaN micro-LEDs for near-eye displays[J]. Advanced science, 2025, 12(40): e06784 doi: 10.1002/advs.202506784
    [9] Liu Y, Wang G, Feng F, et al. Low dislocation density homoepitaxy ultraviolet-A micro-LEDs scale down to 3 μm[J]. IEEE Electron Device Letters, 2024, 45(4): 641−644 doi: 10.1109/LED.2024.3368513
    [10] Junho B, Yuseop S, Hyungyu Y, et al. Quantum dot-integrated GaN light-emitting diodes with resolution beyond the retinal limit[J]. Nature Communications, 2022, 13(1): 1862−1862 doi: 10.1038/s41467-022-29538-4
    [11] Du Z, Fang A, Tang P, et al. Photoluminescence intensity enhancement of nanorod micro-LEDs via localized surface plasmon coupling[J]. Journal of Physics D: Applied Physics, 2024, 58(5): 055105 doi: 10.2139/ssrn.4828628
    [12] Zhang S, Li W, Wang K, et al. Noncarrier injection mode for realizing one line-to-three LEDs driving method[J]. IEEE Transactions on Electron Devices, 2024, 71(4): 2486−2490 doi: 10.1109/TED.2024.3369578
    [13] Li W, Wang K, Li J, et al. Working mechanisms of nanoscale light-emitting diodes operating in non-electrical contact and non-carrier injection mode: modeling and simulation[J]. Nanomaterials, 2022, 12(6): 912−912 doi: 10.3390/nano12060912
    [14] Li W, Wang K, Liao Y, et al. Device simulation on GaN-LED operating in noncarrier injection mode for performance improvement by enhancing the tunneling effect in multiquantum wells[J]. Advanced Electronic Materials, 2023, 9(8): 202300298
    [15] Zhou H, Wang K, Ji X, et al. High resolution micro-LED arrays using Au-Sn flip-chip bonding[J]. IEEE Transactions on Electron Devices, 2023, 70(SI6): 3140−3144 doi: 10.1109/ted.2023.3268628
    [16] Hu Z, Liou Ch, Tsou C, et al. Micro-cantilever array with electroplating tin bumps for flip-chip bonding technology[J]. IEEE Transactions on Components, Packaging and Manufacturing Technology, 2023, 13(12): 2040−2045 doi: 10.1109/TCPMT.2023.3339767
    [17] Yang Z, Fu H, Wang K, et al. Au-In/polymer hybrid bonding and reliability of 1700 PPI micro-LED device[J]. IEEE Transactions on Electron Devices, 2025, 72(7): 3646−3652 doi: 10.1109/TED.2025.3568751
    [18] Yu J, Wang Q, Wu H, et al. Indium-based flip-chip interconnection by electroplating method for superconducting quantum 3D integration architecture[J]. IEEE Electron Device Letters, 2024, 45(10): 2021−2024 doi: 10.1109/LED.2024.3441615
    [19] Tang X, Huang X, Lang T, et al. Active-matrix TFT driven GaN blue micro-LED display realized with electroplated copper-tin-silver micro bumps-based bonding structure[J]. Journal of Alloys and Compounds, 2025, 1010: 177695−177695 doi: 10.1016/j.jallcom.2024.177695
    [20] Li Y, Lee Y, Wu Z, et al. Effect of Ag addition on the mechanical properties of Cu/Ni/Sn/Ni/Cu microbump with a sub-10 micron bump thickness[J]. Journal of Materials Science: Materials in Electronics, 2024, 35(28): 1839 doi: 10.1007/s10854-024-13559-4
    [21] Lucas T j, Biesecker J P, Doriese W B, et al. Indium bump process forlow-temperature detectors and readout[J]. Journal of Low Temperature Physics, 2022, 209(3-4): 293−298 doi: 10.1007/s10909-022-02728-6
    [22] Tian W, Ma Z, Cao X, et al. Application of metal interconnection process with micro-LED display by laser-assisted bonding technology[J]. Journal of Materials Science: Materials in Electronics, 2023, 34(35): 2253 doi: 10.1007/s10854-023-11549-6
    [23] He X, Liu Z, Cai J, et al. Characterization of stencil printing parameters for fine pitch wafer bumping[C]. 2014 15th International Conference on Electronic Packaging Technology, Chengdu, China, 2014, 80−85
    [24] Tian L, Lin C, Pan K, et al. Electroless deposition of 4 μm high Ni/Au bumps for 8 μm Pitch interconnection[J]. ACS Applied Electronic Materials, 2022, 4(10): 4966−4971 doi: 10.1021/acsaelm.2c00974
    [25] Lu Y, Lin C, Tian L, et al. Electroless deposition of high-uniformity nickel microbumps with ultrahigh resolution of 8 μm pitch for monolithic micro-LED display[J]. Materials Science in Semiconductor Processing, 2024, 175: 108263 doi: 10.1016/j.mssp.2024.108263
    [26] Ahn S. G, Oh J H, Jeon G J, et al. A study on improvement and extension of fine-pitch micro-bump interconnects technology: new metallurgy & flux-less oxide-removal laser assembly[C]. 2024 IEEE 74th Electronic Components and Technology Conference (ECTC), USA, 2024, 556−562
    [27] Fritzsch T, Kavianpour F, Rothermund M, et al. Investigation of low temperature bonding process using indium bumps[J]. Journal of Instrumentation, 2018, 13(11): c11007 doi: 10.1088/1748-0221/13/11/C11007
    [28] Wu D, Tian W, Wang C, et al. Research of wafer level bonding process based on Cu–Sn eutectic[J]. Micromachines, 2020, 11(9): 789−789 doi: 10.3390/mi11090789
    [29] Tan B, Liang J, Lai Z, et al. Electrochemical deposition of copper pillar bumps with high uniformity[J]. Journal of Electrochemistry, 2022, 28(7): 2213004−2213004
    [30] Luo C, Lin C, Ye J, et al. Electroplating of Cu/Sn bumps with ultrafine pitch and high uniformity for micro-LED interconnection[J]. Journal of Materials Science: Materials in Electronics, 2024, 35(12): 878 doi: 10.1007/s10854-024-12645-x
    [31] Jiang J, Yang T, Ye J, et al. 3175 PPI micro-LED arrays with FHD-resolution fabricated via electroplating Cu-SnAg bump bonding technologies[J]. Materials Today Communications, 2025, 48: 113624−113624 doi: 10.1016/j.mtcomm.2025.113624
    [32] Shi Y, Wang Z, Zhang H, et al. Transient-liquid-phase bonding of granulated Cu-Sn bumps with a 4 μm fine Pitch[J]. IEEE Transactions on Electron Devices, 2023, 70(2): 683−688 doi: 10.1109/TED.2022.3227895
    [33] Wang Z, Shi Y, Wang Z, et al. Low temperature Cu-Cu bonding using an intermediate sacrificial Sn layer[J]. IEEE Electron Device Lett, 2023, 44(1): 116−119 doi: 10.1109/LED.2022.3221375
  • 加载中
图( 7) 表( 1)
计量
  • 文章访问数:  83
  • HTML全文浏览数:  83
  • PDF下载数:  1
  • 施引文献:  0
出版历程
  • 收稿日期:  2026-06-23
  • 刊出日期:  2026-09-30

面向超高分辨微显示的金属凸点制备工艺研究

摘要: 超高密度微纳显示器件对互连凸点提出了极小间距、高均匀性的严苛要求。本文以电化学沉积为核心工艺,结合紫外激光直写技术制备超细间距铜(Cu)金属凸点阵列。实验优化光刻工艺以获得高分辨率微孔掩模,采用硫酸铜酸性电镀液体系进行生长,探究电流密度、沉积时间等参数对凸点形貌、高度均匀性、内部结构及界面结合性能的影响。最终实现了中心间距2 μm的超高密度凸点的高效制备,阵列尺寸达到5000 × 5000,凸点高度可达2 μm,阵列高度不均匀性低至2.92%。所得铜凸点阵列表面形貌光滑有序、无短路桥连,内部结构致密无孔洞及杂质等缺陷,去除冗余种子层后仍保持稳定结构。基于该工艺,在氮化镓发光二极管(GaN-LED)外延片上制备并成功实现了250 × 250阵列发光,验证了实现12700 PPI像素密度的可行性。本研究或将为超高分辨率微显示器件的互连键合技术与高效发光器件的研发与产业化应用提供参考。

English Abstract

  • Micro-LED由于其高发光效率、高对比度以及超长寿命与稳定性等突出优势,被广泛认为是最具发展潜力的下一代显示技术[1-11]。像素密度的不断提高是当前Micro-LED发展的一大关键方向,这可以从视觉上获得更加清晰、更加准确真实的信息,并可以向AR、VR及MR等领域发展。随着对高像素密度的要求,也意味着显示需要向更小型化、更高度集成化的趋势前进[12-14]。即要求芯片间的超高互连密度,这对于微型显示技术键合工艺提出了新的挑战[15-17]。在考虑高密度互连的同时,还应兼顾高电导率与高结构稳定性。利用导电性能和机械性能优异的金属凸点是解决该技术难题的有效途径。

    近年来,国内外研究人员对金属凸点的制备及键合进行了诸多研究,包括锡[16]、金[15,17]、铟[17,18]、铜[19]、银[20]等金属材料,推动Micro-LED的不断发展。目前用于金属凸点制备的方法包括热蒸发法[21,22]、丝网印刷法[23]、化学法[24-26]等。然而,不同的制备方法目前都面临一些亟待解决的难题。热蒸发法要求高真空的工作环境,并且材料损耗大,沉积速率慢,高昂的成本使其难以在工业上更大规模进行。此外,对于间距亚10 μm的凸点制备而言,热蒸发法存在后续光刻胶难以去除的难题。而对于丝网印刷法,尽管其工艺简单,但只适用于低密度、大尺寸的凸点制备,难以满足当前显示技术的高像素密度需求。化学法具备工艺相对简单、成本低廉以及速率快的优点,以及能够满足亚10 μm尺寸的制备,这在一定程度上是更优异的工艺方案。化学方法包括化学沉积法和电化学沉积法,化学沉积法需要催化材料进行反应催化,比如金属自催化等,这意味着该方法生长的厚度有限,并且控制厚度相对较难。电化学沉积法则是在外加电流条件下,使金属离子在阴极处还原为单质并沉积,一般可以通过控制沉积时间或者工作电流等参数改变厚度。但与此同时,电化学沉积法同样面临一系列难题,如边缘电流效应以及溶液环境中的离子分布不均匀引起的厚度不均匀,仍需要进一步的探索。

    Fritzsch T等[27]利用电化学沉积法后热回流制备直径的平均值为30 μm,高度为21 μm的高均匀性铟金属凸点,该凸点具有优良的导电性,能够满足微芯片的电互连要求。Tian等[28]利用电化学沉积法,通过控制电流密度及添加剂浓度获得了高度均匀性、中心间距为60 μm、直径40 μm的铜/锡凸点,并且研究了一种圆片级高密度不可逆凸点共晶键合技术,良率测试达到100%。Tan等[29]通过电化学沉积制备了高均匀性铜柱凸点,在10 A/dm2电流密度下制备了中心间距150 μm,直径80 μm,高度50 μm的高均匀性铜金属凸点。在亚百微米级凸点制备工艺中,电化学沉积法无疑是一种优异的替代方案。在10 μm节距以下,研究人员同样对于电化学沉积金属凸点进行了诸多探索。Yu等[18]对电化学沉积铟凸点的过程中,发现当凸点的尺寸不断减小时,凸点阵列的均匀性会逐渐恶化,这对于高均匀性的工艺要求是一个不好的消息。Luo等[30]在间距8 μm的铜/锡凸点的电化学沉积制备中,研究了阴阳极间距、电镀液搅拌速度及电流密度对凸点形貌和均匀性的影响,实现了1920 × 1080的高均匀性和表面光滑的凸点阵列。Jiang等[31]通过等离子体处理提高光刻胶表面的润湿性,电镀制备直径5 μm,间距8 μm的铜凸点。Shi等[32]采用电化学沉积和回流焊法结合,将颗粒状锡层代替传统的连续锡层,成功地实现了直径为2.9 μm、间距为4 μm的细间距铜−锡凸点键合,键合成品率高且具有较低电阻率。

    目前,细间距金属凸点制备技术已积累诸多研究成果。随着超高密度显示产业的发展,器件互连端对凸点节距的微型化需求日益迫切,然而针对超小尺寸、超高密度金属凸点的进一步研究仍相对匮乏。鉴于此,本文采用激光直写光刻工艺完成精细图案化制备,再通过电化学沉积实现凸点结构生长。实验探究了多尺度高密度图形的光刻工艺适配性,讨论了电流密度、沉积时间等参数对微凸点形貌特征的调控规律。实验结果表明,该方案可实现中心间距2 μm的铜凸点批量制备,样品形貌均匀、电学性能优良且结构稳定,可为超高像素密度(>10000 PPI)微显示器件的互连键合工艺奠定技术基础。

    • 本工作主要实验步骤如图1所示。制备步骤主要包括基底处理、种子层沉积、光刻胶薄层制备、曝光显影、电化学沉积和光刻胶去除等。

    • 该实验使用起伏在纳米级尺度的低粗糙度玻璃基底,为了保证基底表面的洁净以减少表面污渍对实验造成的不良影响,使用超声清洗机对基底材料进行清洗处理。先是使用乙醇超声5 min以去除油性有机物等杂质,后续使用去离子水超声3 min去除一般杂质和乙醇残留。此外,为了改善基底表面活性不足的问题,对其进行时长10 min的O2等离子处理,利用高能激发的氧等离子体轰击基底表面,使表面化学键断裂形成高能状态,提高表面反应活性,保证后续实验的顺利进行。

      利用高真空热蒸发沉积设备在经过上一步洁净处理的基底上沉积厚度约200 nm的铜金属层。该金属层在实验中扮演两个重要作用:一是作为后续电化学沉积生长的附着种子层;二是作为导电连接层,为电化学反应提供良好的导电通路。因为考虑到后期涉及到种子层去除相关步骤,为避免繁琐的工艺及较高成本,本研究没有额外沉积阻挡层等功能层材料。

    • 将生长好金属种子层的基底材料经过洁净度处理,利用溶液旋涂法将RZJ-304型正性光刻胶在基底上旋涂成膜。成膜过程旋转速度设定为6000 r/min,旋涂时间为30 s,制备厚度2 μm的均匀薄膜。并将样品基底置于100℃恒温条件下进行90 s退火处理,将光刻胶中的溶剂蒸发,使光刻胶定型,同时增强与基底之间的附着性,保证图案化工艺良好进行。

      本次研究使用无掩膜激光直写光刻法(数字微纳光刻系统Miscan-200)进行图案化制备。与普通光刻不同,无掩膜激光直写光刻不需要使用掩膜板,可以直接将设计好的图案转移到基底上,如图1(Ⅳ)所示。本研究使用主要成分为四甲基氢氧化铵(TMAH)水溶液的ZX-238碱性显影液进行显影刻蚀,显影时间设定为75 s。最后在120℃条件下进行加热温度120 s、时间5 min的坚膜处理步骤,蒸发残留的液体,提高光刻胶的抗腐蚀性。

      本研究对光刻工艺参数进行一系列探索优化,目的是为了获得分辨率更高的图案化阵列,主要对工艺所需的曝光剂量大小进行了系统分析。

    • 本研究使用电化学沉积法生长铜金属凸点,实验装置如图2所示。利用电化学沉积法进行金属的沉积生长相比于溅射沉积等速率更快,成本更加低廉,并且在后续的光刻胶去除工艺中具备明显的优势。本研究采用酸性硫酸铜电镀液体系生长铜金属凸点。电镀液的具体组成如表1所示,220 g/L CuSO4·5H2O、35 g/L H2SO4、30 mg/L Cl−、200 mg/L聚乙二醇(PEG-6000)、1 mg/L聚二硫二丙烷磺酸钠(SPS)和3 mg/L健那绿B(JGB)。其中,CuSO4·5H2O为阴极沉积提供Cu2+。H2SO4用于维持镀液酸性、提高溶液电导率并降低欧姆压降。Cl−有助于铜阳极均匀溶解,并可与PEG协同调控铜的沉积过程。PEG-6000作为抑制剂,通过在阴极表面形成吸附层减缓铜的过快沉积,提高凸点高度均匀性。SPS作为加速剂,可促进Cu2+还原及微孔内部铜沉积。JGB作为整平剂,优先吸附于表面突起及局部高电流密度区域,抑制这些位置的铜沉积,从而进一步改善凸点顶部的平整度与表面质量。

      沉积过程中使用直流输出电源,通过外加变阻器辅助精准控制输出电流大小。当外加电流时,阳极铜金属发生如式(1)所示的化学氧化反应:

      阴极样品处发生如式(2)所示的化学还原反应:

      在标准状态下,Cu2+的标准电极电势(+0.3419 V)远高于H+的(0 V),在电场作用下Cu2+会优先还原析出;并且由于我们使用的电流密度相对较低,电荷基本被用于铜的氧化与还原,一般认为不会发生析氢反应等副反应,或者认为这些反应与主反应相比过于轻微,对实验基本无影响,故忽略不计。在正式电沉积之前,对样品进行时长5 min的氧等离子表面处理。离子处理能够显著改善基底材料和光刻胶对水的亲水性,从而使电镀液与光刻胶微孔充分接触,提高沉积中的均匀性等[23,31]。

      为了获得均匀性更高、表面形貌良好的金属凸点,本研究对电化学沉积步骤工艺进行一系列的探索优化。通过优化改变电流密度、沉积时间等参数,探索最佳制备工艺条件。

    • 为满足后续物性表征与微观观测需求,需完成薄层光刻胶的剥离去除工序。本实验选用以N-甲基吡咯烷酮(NMP)为主要组分的溶液开展光刻胶脱除,将试样置于该剥离液中恒温浸泡3 min,使NMP渗入光刻胶高分子链间隙,有效瓦解其交联网络结构。

    • 金属凸点电镀成型后需去除多余导电种子层,首要目的是避免整片晶圆表面连续分布的种子层将相邻凸点、焊盘及布线相互连通,进而引发电路短路造成芯片报废;同时可保障微米级高密度凸点阵列之间的介质绝缘隔离效果,杜绝残留金属层引发的漏电与信号串扰问题,保证器件基础电学性能稳定。因此仅保留凸点正下方UBM及功能性种子层、彻底剔除外围冗余金属,既能够实现各凸点独立电气互连的设计初衷,也可保障芯片长期服役过程中无漏电、短路及结构脱落等失效风险,满足封装器件的设计规范与长期可靠性要求。

      本文使用电感耦合等离子刻蚀(ICP,Mill200)工艺去除凸点下铜种子层,保证种子层均匀去除的同时尽可能减少对凸点产生损伤。

    • 本研究使用台阶仪获取薄膜厚度,通过改变相关参数制备一定厚度的膜层。使用3D激光显微镜(LEXT OLS4100)、光学显微镜等表征图案化和金属凸点的表面形貌以及高度等。同时利用扫描电子显微镜(SEM)和聚焦离子束切割(FIB)协同表征金属凸点的内部结构和轮廓等。通过公式(3):

      计算凸点整体的不均匀性。以及公式(4):

      计算表征凸点轮廓平坦度。将样品划分为3x3阵列区域,每个区域分别测量7个样品点并统计得到该区域样品的平均高度,取其中最值为样品中的高度最大值($ {H}_{\max } $)和最小值($ {H}_{\min } $),再以9个区域平均高度作为统计单元,计算样品整体平均值($ {H}_{\text{average}} $),通过公式(3)计算其高度不均匀性。利用FIB切割后分别测量凸点的左($ {H}_{\text{left}} $)、右($ {H}_{\text{right}} $)两肩高度,以及几何最高点的高度($ {H}_{\max } $),由公式(4)计算得到其轮廓不均匀性。

    • 高分辨率的图案化制备是实验的关键环节之一,同时制备深宽比足够大、关键尺寸均匀性高且间距满足实验要求的高密度微孔阵列也是目前实验室中的一大工艺难点。本研究对激光直写光刻工艺曝光剂量进行了探索优化,旨在制备高精度、高均匀性微米级图案阵列。不同型号光刻胶对紫外光的敏感程度有所不同,通过改变曝光剂量制备相同图案,对比得出最优工艺。曝光使用图案为直径1 μm,中心间距2 μm的圆孔矩形阵列。

      本实验采用数字微纳光刻系统Miscan-200,并使用50×聚焦物镜进行图案化制备。在保持物镜、光源功率及其他曝光条件不变的情况下,系统设定的曝光频率与实际曝光剂量呈负相关关系。通过测量不同频率条件下的曝光剂量,并对实验数据进行函数拟合,如图3(i)所示,并得到曝光剂量与曝光频率之间的经验换算关系:

      其中,E(f)为曝光剂量,单位为mJ/cm2,f为系统设定的曝光频率(kHz)。将曝光频率从65 kHz开始,每间隔5 kHz取一个参数进行样品图案化,根据上述拟合方程,当曝光频率分别为65、70、75、80、85、90、95和100 kHz时,对应的曝光剂量依次约为722.2、683.5、647.9、614.6、582.8、552.1、522.2和493.0 mJ/cm2。使用3D激光显微镜(LEXT OLS4100)进行扫描测量,得到如图3(a)-(h)所示高度图像,并测量图案微孔的直径及高度关系,如图3(j)-(k)所示。

      从图中可以发现,图案化微孔的直径及微孔高度都随着频率的减小而有所增大,即随曝光剂量升高而增大。图案化必须考虑两个关键问题:一是光刻胶是否刻蚀完全,曝光区域底部光刻胶不能留有残留,否则无法形成电连接通路。二是孔径大小是否满足实验关键尺寸要求,其中关键的一点是不能出现桥联,否则会出现短接现象造成器件失效。因此我们在兼顾二者的情况下,认为深宽比是一个重要的参考指标,图3(k)给出了不同曝光频率下的深宽比数据。可以看出在70 kHz条件下深宽比较高(1.26),且该条件下微孔深度足够(2.07 μm),所以以该参数为后续工艺制备。

    • 为了探究超细间距微凸点高度及形貌随电镀时间变化的趋势,本次实验采用4 mA/cm2的工作电流密度进行铜凸点制备,并且该实验过程中阴、阳极间距固定为8.5 cm。对电镀时间分别为2 min、4 min、6 min、8 min和10 min下生长得到的凸点形貌进行表征,如图4所示。分析发现,当沉积时间较短时,凸点高度随时间增长更加迅速,沉积速率约为0.35 μm/min,并且在4 min时达到约1.4 μm的高度。与其他凸点生长的方法相比较,该方法的凸点生长速率是相当快速的,而化学镀生长速率约0.1 μm/min[21],蒸发、溅射沉积生长每分钟仅生长数纳米[21-33]。当时间大于4 min即高度超过1.4 μm之后,明显可以看出凸点高度随时间的变化速率有所下降。并且发现在沉积2 min后生长得到的凸点直径略小于沉积时间较长的样品。

      为了更好地获得所制备铜凸点的整体轮廓及内部形貌,对不同时间下制备得到的样品进行FIB切割并借助SEM对切面形貌进行观察。从横截面我们可以发现凸点内部结构紧密,没有明显的裂纹和孔洞存在。随着凸点高度的增加,内部形貌保持基本一致且良好。优异的内部形貌表明沉积过程中形核速率适中,晶格缺陷少。经测量并由公式(4)计算了不同沉积时间下的顶部轮廓不均匀性,如图4(l)所示。可以看出,在沉积时间为2 min时,轮廓不均匀性高达58.39%,随着时间增长即凸点高度的增加,轮廓不均匀性逐渐降低,当沉积10 min时轮廓不均匀性降低到13.72%。从测量数据及截面形貌图上可以看出,凸点轮廓最高点几乎位于其中心位置,两侧高度大致相等且低于中心位置,从而使凸点顶部整体上呈现椭圆顶状。因此认为该现象主要是由光刻胶的疏水性造成的,即光刻胶对电镀液的浸润性仍然达不到使凸点表面趋于平坦化的要求。图案化微孔内光刻胶与电镀液之间的不完全浸润使得电镀液汇聚在孔洞中部,金属离子的还原沉积首先在中部区域开始,并逐步促使电镀液向四周扩散直至整个微孔底部与镀液紧密接触,这导致生长的凸点中部高度高于边缘且在较短时间下直径有所降低,后期实验仍然需要进一步改善。

    • 在铜凸点的电化学沉积制备工艺中,工作电流密度是一项关键工艺参数,其取值对凸点的高度均匀性与表面形貌具有显著调控作用,相关影响规律一直是该领域研究的重点。相比于大尺寸、低密度排布的凸点结构,小尺寸、高密度集成的金属凸点在相同沉积条件下往往表现出更低的沉积高度,由此引发的高度不均匀问题更为突出。因此,亟需建立更为精准的工艺调控策略以实现高密度微小凸点在生长过程中的均匀且可控制备。本文设置工作电流密度分别为2 mA/cm2、4 mA/cm2、6 mA/cm2、8 mA/cm2和10 mA/cm2,并且通过在2 min-4 min时间范围内调节不同沉积时间,控制凸点最终高度在一定范围内。图5给出了在不同工作电流密度下生长得到的凸点形貌图像。

      凸点顶部光滑平整的形貌是决定芯片互连键合良率的关键评价指标之一,对保障器件优异的导电连通性、可靠的机械支撑性及长期服役稳定性均具有至关重要的作用。由图5所示的不同电流密度下的扫描电子显微镜(SEM)图像表征结果可见,所制备的金属凸点整体呈现出光滑致密的表面形貌,顶部区域无明显的不规则凸起、枝晶或粗糙结构。这表明在本实验工艺条件下,金属凸点具有优异的结晶质量与细小均匀的晶粒尺度。同时,对比不同沉积电流密度下的样品可以发现,凸点表面结晶形貌未呈现显著差异,说明工艺参数在该范围内对表面微观结构的影响比较有限。

      此外,凸点的高度均匀性同样是金属凸点制备重要指标之一。图5(k)给出了各组样品凸点高度分布箱线图与高度不均匀性曲线。从图中可以看出随着电流密度增大,样品不同区域凸点高度分布离散程度加剧,高度极差逐渐增大。并且可以发现高度不均匀性随电流密度的减小而呈降低的整体趋势。该实验结果与先前的研究结论是一致的,即电流密度越小,电镀液体系内电流分布越均匀,不同区域沉积速率越稳定。值得注意的是,在电流密度为4 mA/cm2和2 mA/cm2时凸点高度不均匀性仅为3.41%和2.92%,这是满足芯片封装和Micro-LED键合技术基本要求的(<5%)[31]。

      利用聚焦离子束精准切割后获得的SEM截面形貌,用于系统表征与定量评估不同电流密度下金属凸点轮廓的均匀性水平以及内部结构质量,如图5(l)所示。可以发现,各组样品的轮廓不均匀性未随电流密度变化呈现出显著规律,说明在本实验所选取的工艺区间内,电流密度对凸点宏观轮廓均匀性的调控效果有限。从截面微观结构进一步分析可见,在本研究电流密度范围下沉积制备的金属凸点内部均组织致密,无明显孔隙、微裂纹及杂质等缺陷,体现出良好的结晶取向与致密度。同时,不同电流密度条件下凸点与底部种子层界面结合完整、接触紧密,未观察到界面空洞、缝隙或剥离现象,界面结合状态优异。上述结构特征为凸点提供了稳定的内部承载结构与高效的电荷传输通道,在实际应用中可实现优异的导电性能与可靠的机械支撑能力。

    • 为了去除铜种子层,使用电感耦合等离子刻蚀(ICP)工艺进行种子层的刻蚀。其原理为氩气在高频强电场作用下被激发并加速形成高能氩等离子体(Ar+),垂直轰击样品表面,表面铜在高能离子轰击下溅射去除,如图6(a)。如图6(b)-(d)所示是种子层未去除时的样品形貌,图6(e)-(g)是对应的样品经ICP刻蚀去除铜凸点下金属种子层后的形貌。对比发现相邻凸点之间的铜金属层被良好去除,并且刻蚀过程并不会对凸点造成明显破坏。这表明在此工艺条件下制备的超高密度金属凸点能在ICP刻蚀去除种子层之后完好保留与于基底背板上,保证在驱动过程中的稳定工作及不会出现电流短路情况。同时对比前后高度发现凸点高度有轻微的下降,这是因为ICP对样品整体进行非选择性刻蚀,合理控制刻蚀时间能够使种子层完全去除的同时尽可能减少对凸点本身以及基底的损伤,使损伤在可接受范围。

    • 为了验证高密度凸点间种子层的有效去除,以及本文工艺在超高密度器件中的应用可行性,将铜凸点直接生长于氮化镓外延LED(GaN-LED)发光芯片上,制备步骤同上文,如图7(b)所示。在铜凸点制备完成并去除种子层后,继续利用ICP刻蚀氮化镓层。在这个过程中,铜凸点可作为硬掩模,其下方的氮化镓层被保护不会出现损伤,相邻凸点之间的区域则会被垂直向下刻蚀,最终形成柱状GaN-LED阵列结构,如图7(c)所示。之后用旋涂法将光刻胶在样品表面制备成均匀薄层,聚合物的高流动性会均匀填充到凸点之间的微小空隙中。提高凸点稳定性以及保证相邻凸点之间的电隔离是填充光刻胶的两个主要作用,如图7(d)所示。但该填充方案不可避免会在凸点表面同样附着聚合物材料,实验中需要去除掉表面聚合物使得铜凸点暴露,形成完整的导电通路。利用高能等离子对填充聚合物后样品表面进行轰击,其能使聚合物分子溅射,而对铜金属几乎没有损伤。在控制一定处理时长后,表面聚合物明显减薄,直至铜凸点暴露于外界时停止轰击,因此可以保证金属凸点顶部未被聚合物覆盖且间隙依然完整填充,如图7(e)所示。在金属凸点暴露之后,通过热蒸发镀膜沉积一定厚度的银电极,将相互独立的GaN-LED柱并联以便后续驱动。

      最后在外加直流电场驱动下实现了250 × 250像素阵列发光,像素密度高达12700 PPI,如图7(g)-(i)所示。在高倍显微镜观察下,可以明显看出发光区域由独立的像素点构成,如图7(i)所示。每一个发光像素点由一个单独铜凸点进行驱动,且每个像素点具有清晰分明的边界,这与超高密度成像技术高度契合。尽管器件各区域发光强度不均匀,但是我们证明了这种相对简单、低成本的制备以及驱动方案在超高像素密度发光器件中的可行性。

      针对器件在直流驱动下呈现的发光不均匀现象,结合器件制备流程分析,该现象最可能与凸点顶部绝缘层去除不充分及其引起的电流注入差异有关。光刻胶旋涂过程中产生的初始厚度差异,以及等离子体处理区域能量密度和刻蚀速率的空间非均匀性,均可能导致部分区域的绝缘层未被完全去除,使铜凸点顶部残留薄层绝缘介质。该残留层会影响后续金属电极与铜凸点之间的直接接触,造成不同像素的接触电阻和电流注入效率存在差异,进而表现为局部像素亮度降低或不能有效发光。

      后续可从以下方面改进:首先,优化光刻胶黏度、旋涂参数及固化条件,并对不同区域的绝缘层厚度进行测量,以提高初始膜厚均匀性。此外,采用低功率分步等离子刻蚀、样品旋转及刻蚀终点监测等方法,能有效提高绝缘层减薄和凸点暴露过程的均匀性。在刻蚀后,可引入具有全局平坦化能力的化学机械抛光工艺,使绝缘层均匀减薄并充分暴露各区域的铜凸点。同时需要优化抛光压力、时间及终点控制,以减少凸点损伤、凹陷和过度抛光。对于电极与电流扩展结构,可进一步优化金属沉积均匀性、界面清洁工艺及电极结构,以降低片内串联电阻与接触电阻差异。

    • 本文围绕超细间距微金属凸点可控制备开展探究,采用电化学沉积法,通过精准调控沉积时间、电流密度等核心工艺参数,成功制备出中心间距低至2 μm,分辨率可达5000 × 5000的铜金属凸点阵列,所得凸点表面形貌光滑规整、内部晶体结构致密均匀,具备优异的结构均一性,高度不均匀性仅为2.92%。通过电感耦合等离子体刻蚀工艺,实现凸点下方冗余金属种子层的完全去除,同时完好保留高精度凸点阵列的完整结构,有效避免了刻蚀工艺对微凸点形貌与力学稳定性的损伤。基于上述制备工艺,最终成功实现250 × 250阵列尺寸的GaN-LED像素阵列制备并驱动发光,器件发光像素密度高达12700 PPI。本研究充分验证了实验室条件下超细间距微金属凸点可控制备的可行性,并证实其在超高像素密度显示领域的应用潜力,可为下一代超高密度微型显示技术的发展与封装工艺革新提供重要的实验依据与技术参考。