With the continuous development of electronic technology, flexible electronic devices prepared by gel-based materials are receiving more and more attention [1-3]. According to the conductive mode, they are mainly classified into electronic conductive gels and ionic conductive gels. Electronic conductive gels are materials that conduct electricity by free electrons (conducting nanofillers carbon nanotube, graphene, MXene, etc. or composite conducting polymers polyaniline, polypyrrole, etc.) [4-6], while ionic conductive gels conduct electricity by free ions [7-9]. Due to good electrical conductivity and biocompatibility, hydrogels have been widely used in sensors [10-12], electronic skin [13-15], light-emitting devices [16-18], etc. However, hydrogel is easy to lose water in open air, which makes the hydrogel crumple, and the flexibility and tensile properties of hydrogel will fall sharply [19-21]. In addition, at low temperature below freezing point, the water in hydrogel will freeze, causing the hydrogel to lose its flexibility and conductivity [22-24]. Ionogels are based on ionic liquids. Ionic liquid is a liquid composed of only ions, which is actually a salt with a very low melting point and non-volatile components, so ionogels are widely used in flexible electronic devices and other fields [25-27]. However, ionic liquids are expensive, hard to prepare and of poor biocompatibility, which are the most important factors hindering the application of ionic conductive gels [28-30].
A deep eutectic solvent (DES) is a mixture composed of hydrogen bond donor (HBD) and hydrogen bond acceptor (HBA) in a molar ratio of 2:1, where the hydrogen bond acceptor is usually a quaternary ammonium salt. DES has a melting point significantly lower than that of each component and is usually in liquid form at room temperature. As excellent alternatives to ionic liquids, DESs are cost-effective, easy to prepare, biocompatible and non-volatile, and widely used in the field of green chemistry [31-33]. The preparation of eutectogels has been widely reported. Guo et al. initiated the polymerization of acrylic acid in a deep eutectic solvent composed of choline chloride, glycerol, diethylene glycol, ethylene glycol and urea, and obtained ionic conductive gels based on polyacrylic acid deep eutectic solvents, which had high stretchability ( > 1000%), high electrical conductivity (1.26 mS/cm), high adhesion (~100 N/m), and good resistance to drying and freezing [34]. Yan et al. obtained an eutectogel based on poly(vinyl alcohol)/poly(acrylic acid) via photopolymerization by mixing acrylic acid with poly(vinyl alcohol) in a deep eutectic solvent consisting of choline chloride and ethylene glycol, which had tensile strength of 2.6 MPa, fracture strain of 680%, and toughness of 8.39 MJ/m3, and can recover mechanical performance in 600 s after tensile-recovery cycle at a strain of 100%. The eutectogel exhibited good sensitivity over a wide strain range (1%-300%) and maintained highly reproducible response signal over 1000 consecutive tensile-recovery cycles, showing excellent long-term stability and durability [35]. Gao et al. obtained a new deep eutectic solvent by mixing two deep eutectic solvents, acrylamide-choline chloride and choline chloride-glycol, and added 2-acrylamido-2-methylpropane sulfonic acid (AMPS) for polymerization under UV light to obtain an eutectogel with tensile strain of 2300%, fracture stress of 0.21 MPa, electrical conductivity of 0.22 mS/cm, and adhesion strength on copper up to 90 kPa [36]. However, since a DES contains a large number of hydrogen bonds, it inevitably exhibits hydrophilicity and absorbs water from the air, thus affecting the performance of eutectogel [37-39] .
In this work, we first used the quaternization reaction of 1-bromooctadecane and N-dimethylaminopropyl acrylamide to obtain a reactive quaternary ammonium monomer with a hydrophobic chain of 18 carbons, (3-’acrylamidopropyl)octa-decyldimethyl ammonium bromide, which was mixed with choline chloride, acrylic acid and glycerol to obtain a deep eutectic solvent. Then we added 2-hydroxy-2-methylpropiophenone (Irgacure 1173) as photoinitiator and initiated polymerization under UV light of 365 nm to obtain an eutectogel based on polyacrylamide copolymer with long hydrophobic chain. The eutectogel has maximum tensile elongation of 1200%, Young’s modulus of 0.185 MPa, toughness of 4.2 MJ/m3, and electrical conductivity of 0.315 S/m, and the eutectogel can respond sensitively to joint bending. The eutectogel was then placed in an ambience of 25 °C and 60% humidity for 7 days, and the final water absorption rate is 11.7%, which is half of that of the eutectogel without long hydrophobic chains (24.0%). The introduction of long-chain hydrophobic groups not only improves the mechanical strength of the gels, but also greatly improves the moisture resistance of the gels. This work provides a simpler and more effective method for the preparation of eutectogels, which in turn provides a reference for the application of eutectogels in the field of flexible electronic devices.
-
1-Bromooctadecane, N-dimethylaminopropyl acrylamide, and choline chloride (ChCl) were purchased from Shanghai Aladdin Biochemical Technology Co. Ltd. Acrylic acid (AA), glycerol (Gly), hydroquinone, acetone, and ether were purchased from Sinopharm Chemical Reagent Co. 2-Hydroxy-2-methylpropiophenone (Irgacure 1173) was purchased from Shanghai Macklin Biochemical Technology Co. Diallyldimethylammonium chloride and (3-acrylamidopropyl) trimethylammonium chloride (named as C1) were purchased from Sarn Chemical Technology (Shanghai) Co.
The chemicals used in this work were all analytical pure, and all chemicals were directly used without further purification. The water used in the experiments was all deionized water.
-
0.1 mol of N-dimethylaminopropyl acrylamide (156.22 mol/L) and 0.12 mol of 1-bromooctadecane (333.39 mol/L) were added into a single flask. 10 mg of hydro-quinone was added as a polymerization inhibitor to protect the double bond, and 50 mL of acetone was added as solvent. The mixture was stirred for 4 h at 60 °C. The product was evaporated to remove acetone and added in ether for precipitation, then the ether was removed by suction filtration. After being washed three times in ether, the product was placed in a vacuum oven to remove the residual ether. Finally a white powder was obtained, which is (3-acrylamidopropyl)octadecyldimethylammonium bromide (named as C18). The 1H NMR spectrum of C18 is shown in FIG. 1.
-
As shown in Table I, a certain amount of C18, ChCl, AA, and Gly were mixed and 0.25 g of 2-hydroxy-2-methylpropiophenone (Irgacure 1173) was added as a photo-initiator. The mixture was stirred at 60 °C until a homogeneous DES was obtained, then the DES was added to a glass mold sealed by a silastic gasket and polymerized under UV light of 365 nm. The eutectogel was obtained after 5 h. A group of eutectogels were obtained and named as C18-X (X=1–3), and the eutectogel consisting of only ChCl, AA, and Gly was named as C0. Then C18 was substituted by C1 and another group of eutectogels were synthesized and named as C1-X (X=1–3).
-
After preparation, the eutectogel samples were characterized by attenuated total reflectance Fourier transform infrared spectroscopy (Nicolet iN10MX, USA).
-
To evaluate the transparency of eutectogels, the transmission spectra were measured by an ultraviolet-visible spectrophotometer (Shimadzu, UV3700, Japan) with a scan range of 200–900 nm. The samples were 1 mm thick.
-
A differential scanning calorimeter (DSC 214, NETZSCH) was used to investigate the thermal stability of eutectogels. The testing temperature was from −80 °C to 120 °C at a rate of 5 °C/min and then cooled down to −80 °C.
-
The mechanical properties of the samples were tested using the tensile test machine (EZTest, SHIMADZU). In the tensile test, all samples were cut into strips of 12.5 mm × 2 mm × 1 mm, and were tested at a stretching rate of 50 mm/min. In the mechanical compression test, all samples were cylindrical samples of 7.5 mm in radius and 20 mm in height and tested at a compression rate of 50 mm/min. In the tensile loading-unloading cycle test, the stretching rate was 100 mm/min. Young’s modulus was obtained by calculating the slope of the stress-strain curve in the range of 1%–5% strain. The toughness was calculated by integrating the entire stress-strain curve. The dissipative energy was obtained by calculating the area of the hysteresis circle of the loading-unloading curve. The recovery rate was obtained by dividing the dissipative energy for each loading-unloading cycle by the dissipative energy for the first cycle.
-
Tensile adhesion tests were conducted using the tensile test machine (EZTest, SHIMADZU, Japan) to test the adhesion properties on different surfaces of eutectogel samples. The surface substrates selected for this test were glass, silastic, polyethylene, wood, copper, and aluminum. The gel was made into a circular sheet of approximately 1 mm thick with a radius of 7.5 mm, and the surface substrates used for the test was cut into strips of 5 cm × 2.5 cm. The gel was sandwiched between two substrates, and a load of 1 kg was applied to the joint area and kept for 10 min to ensure the gel adhered to the joint area evenly and adequately. Afterwards, the adhesion area was measured again and the tensile adhesion test was performed at a rate of 20 mm/min. The test was stopped when the load reached its maximum and started to decrease. The adhesion strength was obtained by dividing the maximum load by the adhesion area.
-
The dynamic viscoelastic behavior of the eutectogel samples was tested by a rheometer (AR-G2, TA Instruments, USA). The instrument was equipped with an external water circulation system to control the measurement temperature. The tests were performed using a 40 mm diameter plate with a distance of 1 mm between the plate and the test platform. The frequency sweeps of the storage modulus (G′) and loss modulus (G′′) were in the range of 100–0.1 rad/s.
-
The electrical properties of the materials were tested using an electrochemical workstation (Bio-logic VMP-300). The gels were cut into strips (15 mm × 5 mm×1 mm). Electrodes were attached to copper sheets and separately placed on the two sides of the gel to measure the resistance at a voltage of 1 V. The gel strip was subjected to a tensile loading-unloading cycle at a specific strain using the tensile test machine, while the resistance of the gel was measured in real time using an electrochemical workstation. The rate of resistance change of the gel was obtained by dividing the variation of resistance value by the initial resistance value. The conductivity of the gel was obtained by dividing the distance between the electrodes by the resistance value and the cross-sectional area. The gauge factor (GF) of the gel was obtained by dividing the rate of resistance change by the corresponding strain.
-
An empty Petri dish was weighed first, then the gel sample was placed in the Petri dish and weighed, after which the Petri dish with the sample was placed in an intelligent incubator (HWS-50B, Tianjin), with the temperature set to 25 °C and humidity set to 60%. The mass was weighed at regular intervals and the water absorption of sample was calculated. The water absorption was obtained by dividing the increase in the mass of the sample by the original mass of the sample.
-
Contact angle of material surface was measured using a contact angle meter. A tiny drop of water was placed on the surface of the gel using the syringe of the contact angle meter, and the contact angle was measured from the image acquired by the contact angle meter.
-
Via the quaternization reaction of 1-bromooctadecane and N-dimethylaminopropyl acrylamide, we obtained (3-acrylamidopropyl)octadecyl-dimethyl ammonium bromide (C18), a hydrophobic quaternary ammonium monomer with an octadecyl chain, as shown in FIG. 2(a). At room temperature, C18 is white powder. The preparation principle of C18 eutectogel is shown in FIG. 2(b).
Different eutectogels were prepared, as shown in Table I. All C1 and C0 eutectogels have low mechanical strength, while all C18 eutectogels are well formed with certain elasticity, which tentatively suggests that the quaternary ammonium monomers with long hydrophobic chain play a certain role in enhancing eutectogel’s mechanical strength.
We performed ATR-FTIR analysis on C18-1, C18-2, and C18-3, as well as on a controll sample C1-3, and the results are shown in FIG. 3(a). A broad peak at 3318 cm−1 is assigned for the O–H stretching vibration and the one at 1720 cm−1 is the C=O stretching vibration. C18-3 has a peak at 1647 cm−1, which is the stretching vibration of C=C. The peak of C18 eutectogels at this point is not obvious, which indicates the high degree of reaction of C=C. C18 eutectogels have a peak at 2921 cm−1, and the peak of C1-3 at this point is not obvious, which is the asymmetric vibration of C–H of methylene, and the intensity of this peak increases with the content of C18 in eutectogel.
Transparency is an important metric for flexible electronic sensors, allowing visualization of the internal conditions and structure of the device during operation. The UV-visible absorption spectra of the gels in the wavelength range of 200–900 nm are shown in FIG. 3(c), where the transparency of all three gels reaches 70%. The icon covered by the eutectogel C18-2 is clearly visible as shown in FIG. S1 (Supplementary materials (SM)).
In addition, eutectogels should be freeze-resistant as well as heat resistant, which is important for their application as wearable devices under harsh conditions. To evaluate thermal stability of the gels, we performed DSC tests on three samples of eutectogel C18-X in the temperature range of −80 °C to 120 °C, and the results are shown in FIG. 3(b). No peaks appear in the curves, indicating that the gels do not show any obvious phase transition between −80 °C and 120 °C. The gels are thermally stable and can maintain performance well.
-
To characterize the mechanical properties of the eutectogels, we first tested the tensile stress-strain curves of the eutectogel samples and calculated the corresponding Young’s modulus and toughness. From FIG. 4 (a) and (c), we can see that the tensile stresses at break for C18-1, C18-2 and C18-3 are 0.48 MPa, 0.61 MPa and 2.13 MPa, respectively; and the Young’s moduli are 0.031 MPa, 0.185 MPa and 1.62 MPa, while the elongation at break reduces from 2140% to 1200% and 860%. As the molar ratio of hydrophobic monomer C18 increases, the tensile fracture stress and Young’s modulus of the gel increases, while the elongation at break decreases. This is due to the hydrophobic interactions between the hydrophobic side groups on the polymer chains, which act as physical crosslinks in the gels. We also performed compression tests, and the results are shown in FIG. 4(b), which shows that the compression strength of the gel also increases with the increase of hydrophobic monomer. As shown in FIG. S2 (SM), a C18-2 gel sheet with a cross-sectional area of 5 mm2 was able to lift a steel block weighing 500 g even after being twisted and knotted.
We also investigated multiple tensile-recovery cycles of the eutectogel at the same strain. FIG. 5 (a), (b) and (c) show the stress-strain curves of eutectogels C18-1, C18-2, and C18-3 under five tensile-recovery cycles at 200% strain, respectively, and the curve of C18-1 is the most dense and shows a high recovery. We calculated the dissipative energy versus the recovery rate for the three gels, as shown in FIG. 5 (d) and (e). The recovery rate of C18-1 eutectogel with the lowest hydrophobic monomer content decreases from 78.3% to 59.7% at the beginning, while the recovery rate of C18-3 gel with the highest hydrophobic monomer content is only 51.7% at the beginning and decreases to 35.3% afterwards. It can be seen that the recovery performance of the gels gradually decreases as the content of hydrophobic monomer C18 increases. We performed continuous tensile stress loading-unloading tests. FIG. 6(a), (b) and (c) shows the loading-unloading curves of the three eutectogels C18-1, C18-2, and C18-3 at different strains (100%, 200%, 300%, and 400%). Significant hysteresis loops and instantaneous residual strains are observed in the loading-unloading curves, and we further calculated the toughness and dissipative energy of the gels at different strains. As shown in FIG. 6 (d) and (e), at 100% strain, the total toughness of the three eutectogels are 28.0 kJ/m3, 68.4 kJ/m3, and 424 kJ/m3, and the dissipative energies are 8.26 kJ/m3, 31.5 kJ/m3, and 258 kJ/m3, respectively. when the strain reachs 400%, the toughness reach 185 kJ/m3, 260 kJ/m3, and 1279 kJ/m3 and the dissipative energies are 53.7 kJ/m3, 127 kJ/m3, 705 kJ/m3. This indicates that the gels all have very good toughness and dissipative properties.
-
It is of great importance for the laminated use of human body or devices as well as for reuse if the eutectogel also has good adhesion and self-healing properties. Eutectogels have inherently weak adhesion properties due to the presence of multiple hydrogen bonds of glycerol. In addition, both hydrogen bonding and hydrophobic interactions in the eutectogels can provide some adhesion on different substrates. For this purpose, the adhesion of three eutectogels C18-1, C18-2, and C18-3 were tested on six surfaces (glass, silastic, polyethylene, wood, copper, and aluminum), as shown in FIG. 7(e), and the adhesion strength were measured and calculated by a tensile testing machine, the results are shown in FIG. 7 (a), (b), and (c). FIG. 7(d) shows the adhesion strength of the three gels to different surfaces. As can be seen from FIG. 7(d), the variation in the content of hydrophobic monomers in the eutectogel has a greater effect on the adhesion strength for glass, copper, polyethylene, and wood surfaces, while for aluminum and silicone rubber, the difference is not significant.
To study the dynamic properties of the eutectogel, we tested the rheological properties of the eutectogel. As can be seen from FIG. 8, the storage modulus G' of C18-1 and C18-2 is larger than the loss modulus G'' in the frequency scan range of 0.1–600 rad/s, which proves that the samples are always gels. In contrast, the gel-sol transition point of C1-3 as the control sample appeared around 0.1 rad/s, indicating that it changes to a flowing sol state at low frequencies. According to the equivalence principle of high temperature and low frequency in the time-temperature equivalence principle, it is difficult to maintain solid for C1-3 eutectogel at high temperature.
-
Electrical property is one of the most important properties of electronic devices, and quaternary ammonium salts play the role of electrical conductivity in the composition of eutectogels. Considering the mechanical and adhesion properties of the gel, we chose C18-2 to test the electrical properties. Firstly, we tested the electrical conductivity of C18-2. When the electrode is installed, a certain pressure will be applied to the gel, making the gel deformed, which may lead to the change of resistance, the stable value is taken as the resistance value of the gel after the measurement curve is stabilized, and the electrical conductivity of the gel is calculated as 0.315 S/m after several measurements.
We measured the real-time resistance of C18-2 sample at large strains (100%, 200%, 400%, 800%) and small strains (5%, 10%, 20%, 40%, 80%) and at different stretching rate, and obtained the curves of the rate vs. change of resistance with strain, and the results are shown in FIG. 9 (a), (b), and (c). As can be seen in resulted curves, the rates of change of resistance are similar at same strain, and the differences in the rates of resistance change at different strains are all significant. Moreover, for different strains, as the strain increases, the gel is more responsive to the strain. We calculated the gauge factor (GF) of the gel, and the results are shown in FIG. 9(d). The GF of the gel is 2.13 for strains below 200%, and rises to 4.41 and 6.62 for strains of 200%–600% and 600%–1000% respectively. From FIG. 9(c), we can see that as the stretching rate rises, the rate of resistance change gradually decreases from 126% at a stretching rate of 10 mm/min to 44% at 100 mm/min. Considering that there is no obvious sudden decrease in the rate of change of resistance during each stretching cycle, it can be assumed that the rate of change of resistance of the gel is not affected by the stretching rate. Meanwhile, we performed 120 tensile loading-unloading cycles on the C18-2 sample at 200% strain and measured its resistance in real time, and the obtained result is shown in FIG. 9(e), where the resistance change rate gradually decreases from 306% at the beginning to fluctuate around 130% without any obvious abrupt drop.
To investigate the sensing properties of the gel, we conducted a simple sensing experiment by adhering a long strip of C18-2 gel to the joint of the experimenter, bending the joint and measuring the resistance in real time, after which we obtained the sensing curves of the finger joint and metacarpophalangeal joint of the experimenter, as shown in FIG. S3 (a) and (b) in SM. It can be seen that the electrical signal is more sensitive to the gel deformation caused by the joint bending and has a good repeatability.
-
By introducing hydrophobic groups, we tried to reduce the hydrophilicity of the eutectogels containing a large number of hydrogen bonds. We first measured the contact angle of water on eutectogel surface. As shown in FIG. 10(a), the contact angle of C1-3 is only 23.8°, while the contact angles of C18-1, C18-2 and C18-3 are all about 80°, indicating that the introduction of hydrophobic chain increased the hydrophobicity of the eutectogel significantly but still could not make the eutectogels totally hydrophobic.
The absorption of water is a critical issue of the application of eutectogel, for the absorption of water can influence the properties of eutectogel. We placed the eutectogel samples in an intelligent incubator that can maintain temperature and humidity. The temperature was 25 °C and the humidity was 60%. The mass of the samples was measured at regular intervals to calculate water absorption of the samples by the change of mass. After 7 days, the results are shown in FIG. 10(b). The water absorption of C1-3, which did not have hydrophobic groups, finally reached 24.0%. As can be seen from FIG. 10(c), C1-3 performed a clear sol-gel shape due to water absorption, while C18-1, C18-2, and C18-3 with the introduction of hydrophobic groups were able to maintain their shapes with water absorption of 11.0%, 11.7%, and 18.3%, respectively. It was demonstrated that the introduction of hydrophobic groups helped to reduce the water absorption of the eutectogels. C18-2 and C18-3 appear opaque after absorbing water for a period of time, which was probably due to water-induced phase separation.
To investigate influence on properties of the eutectogels after absorbing ambient water, we did conductivity measurement and tensile test on the eutectogels. The samples after placement at 25 °C and 60% humidity were named C18-1′ , C18-2′ , and C18-3′ . The results are shown in FIG. 10(d–f). It can be seen that the conductivity increases and the mechanical strength decreases significantly. However, the mechanical strength is still good and acceptable. So, the hydrophobic chains could not help maintain conductivity and mechanical strength of eutectogels. The main role of the hydrophobic chains was to form physical crosslinking by hydrophobic interaction in eutectogels, which helped enhance mechanical strength and maintain morphology of eutectogels when absorbing water. And the hydrophobic chains significantly reduced the hydrophiliciy of the surface of eutectogels, making it less likely to absorb ambient water.
-
In this work, we synthesized a hydrophobic quaternary ammonium (3-acryl-amidopropyl)octadecyldimethylammonium bromide (C18) with an octadecyl chain by quaternization reaction of 1-bromooctadecane with dimethylaminopropyl acrylamide, and mixed C18 with choline chloride, acrylic acid and glycerol to obtain a polymerizable deep eutectic solvent. An eutectogel C18-X (X=1, 2, 3) with good mechanical properties, electrical conductivity and moisture resistance was obtained by initiating the polymerization of the DES under UV light. In C18-X′ eutectogel, the hydrophobic interactions brought by the introduction of hydrophobic groups act as physical crosslinks, which make the eutectogel perform excellent and adjustable mechanical properties without chemical cross-linking agents. The euctectogel has good tensile properties (860%–2140%), Young’s modulus (0.031–1.62 MPa) and toughness (4.20–10.38 MJ/m3). In addition, the eutectogel has good adhesion properties on surfaces such as glass, silicone rubber, wood, polyethylene plastic, copper, and aluminum. Meanwhile, the eutectogel has good electrical conductivity (0.315 S/m) and sensing properties, and can respond sensitively to joint bending movements of the human body. The eutectogel has good freezing resistance and thermal stability, and compared with normal eutectogel, the moisture resistance of the eutectogel is improved with the introduction of hydrophobic groups. The eutectogel has a water absorption of only 11.7% at 25 °C and 60% humidity for 7 days. This work provides a strategy to improve the environmental stability of eutectogels, which broadens the use of eutectogels in practical applications and may be useful in the design and fabrication of green and inexpensive flexible ionic conductors.
Supplementary materials: The transparency, mechanical and sensing properties of the eutectogel propertie tests and results of C18-2 eutectogel are shown.
Preparation and Characterization of Ionic Conductive Eutectogels Based on Polyacrylamide Copolymers with Long Hydrophobic Chain
- Received Date: 25/04/2023
- Available Online: 27/10/2024
-
Key words:
- Hydrophobic long-chain copolymer /
- Deep eutectic solvent /
- Ionic conductive eutectogel /
- Moisture resistance
Abstract: With the blooming development of electronic technology, the use of electron conductive gel or ionic conductive gel in preparing flexible electronic devices is drawing more and more attention. Deep eutectic solvents are excellent substitutes for ionic liquids because of their good biocompatibility, low cost, and easy preparation, except for good conductivity. In this work, we synthesized a reactive quaternary ammonium monomer (3-acrylamidopropyl)octadecyldimethyl ammonium bromide with a hydrophobic chain of 18 carbons via the quaternization of 1-bromooctadecane and N-dimethylaminopropyl acrylamide at first, then we mixed quaternary ammonium with choline chloride, acrylic acid and glycerol to obtain a hydrophobic deep eutectic solvent, and initialized polymerization in UV light of 365 nm to obtain the ionic conductive eutectogel based on polyacrylamide copolymer with long hydrophobic chain. The obtained eutectogel exibits good stretchability (1200%), Young’s modulus (0.185 MPa), toughness (4.2 MJ/m3), conductivity (0.315 S/m). The eutectogel also shows desireable moisture resistance with the maximum water absorption of 11.7 wt% after one week at 25 °C and 60% humidity, while the water absorption of eutectogel without hydrophobic long chains is 24.0 wt%. The introduction of long-chain hydrophobic groups not only improves the mechanical strength of the gels, but also significantly improves moisture resistance of the eutectogel. This work provides a simpler and more effective method for the preparation of ionic conductive eutectogels, which can further provide a reference for the applications of ionic conductive eutectogels in the field of flexible electronic devices.
首页
登录
注册


DownLoad: