Mengqi Wan, Qian Wen, Mengyi Ci, Wangyang Li, Zhen Zhang. Enhanced Photocatalytic Performance of Anatase TiO2 by Deposition-Precipitation Treatment[J]. Chinese Journal of Chemical Physics, 2024, 37(4): 531-538. doi: 10.1063/1674-0068/cjcp2305055
Citation: Mengqi Wan, Qian Wen, Mengyi Ci, Wangyang Li, Zhen Zhang. Enhanced Photocatalytic Performance of Anatase TiO2 by Deposition-Precipitation Treatment[J]. Chinese Journal of Chemical Physics, 2024, 37(4): 531-538. doi: 10.1063/1674-0068/cjcp2305055

Enhanced Photocatalytic Performance of Anatase TiO2 by Deposition-Precipitation Treatment

  • Corresponding author: E-mail: zzchem@ustc.edu.cn
  • Received Date: 25/05/2023
    Available Online: 27/08/2024
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(5)

Article Metrics

Article views(847) PDF downloads(4) Cited by(0)

Access History

Enhanced Photocatalytic Performance of Anatase TiO2 by Deposition-Precipitation Treatment

Abstract: Deposition-precipitation (DP) method is commonly used to prepare the supported metal catalysts. In this study, the modification effect of the mild DP method on the photocatalytic performance of TiO2 was investigated. The TiO2 samples with DP treatment, as well as Au/TiO2 prepared under the same conditions, showed enhanced photocatalytic performance of the degradation of methylene blue (MB). ·OH generated by photoexcited holes is identified as the main intermediate reactive species during the degradation reaction. X-ray photoelectron spectroscopy (XPS) and Fourier transform infrared spectroscopy (FTIR) show that TiO2(A)-17 after DP treatment has the most amount of surface ${\rm{OH}}_{\rm{ad}}^- $ species. The presence of surface ${\rm{OH}}_{\rm{ad}}^- $ species not only changes the surface zeta potential, favoring the attraction of cationic MB; but also depresses the electron-hole recombination, favoring photodegradation of MB by hole-produced ·OH. An implication of these findings is that the modification of support properties should be taken into account while preparing supported metal catalysts using DP methods.

    • Semiconductor-based photocatalysis provides a promising solution for energy utilization and pollution treatment [1, 2]. Due to its chemical stability, non-toxicity, and low cost, TiO2 has been widely studied in the fields of heterogeneous photocatalysis [3], such as hydrogen production by water splitting, H2O2 synthesis by oxygen reduction reaction, non-fossil fuel synthesis by CO2 photoreduction, organic degradation and disinfection of bacteria [4-7]. To improve the photocatalytic efficiency, metal particles have been deposited on TiO2 to modulate the energy band structures and/or promote the separation of electron-hole pairs [8].

      Deposition-precipitation (DP) method is frequently used for the preparation of highly dispersed metal-supported TiO2 catalyst [9, 10]. In a typical DP process, the soluble metal ions react with hydroxyl ions in a heating solution and the formed small crystallites of metal hydroxides or metal oxides deposit onto the supporting materials. The hydroxyl ions are introduced by the addition of an alkaline solution or by the hydrolysis of urea. Many studies have shown that metal supported on TiO2 by DP methods presents extraordinary catalytic or photocatalytic performance [5, 10, 11]. However, few studies focus on the influence of the DP methods on the TiO2 substrates. Meanwhile, it has been reported that the catalytic performance of TiO2 can be enhanced by harsh conditions, such as the hydrothermal modifications with concentrated alkaline conditions and/or at high temperatures [12, 13].

      In this study, the detailed effect of the mild DP method on the photocatalytic performance of TiO2 was investigated. A series of TiO2 samples were prepared by varying the DP processing time. The TiO2 samples with DP treatment showed enhanced photocatalytic performance of the degradation of MB as well as Au/TiO2 prepared under the same conditions, which was attributed to the change in the number of adsorbed OH groups (${\rm{OH}}_{\rm{ad}}^- $) by DP treatment. The ${\rm{OH}}_{\rm{ad}}^- $ can promote the separation of photogenerated electron (e−) and hole (h+), which in turn enhances the photocatalytic effect.

    II.   EXPERIMENTS
    • The details for the synthesis of Au/TiO2(A)-17 were carried out as follows: HAuCl4·3H2O solution (0.51 mL, 0.1 mol/L) and TiO2 (1.0 g, Shanghai Luoen Reagent, anatase, 99.8%) were added into 100 mL water, and the NaOH solution (0.1 mol/L) was used to adjust the pH value to 8 with vigorous stirring at room temperature. The resulting suspension was stirred for 17 h at 90 °C before being cooled to room temperature. Then, the mixture was centrifuged and the precipitation was washed with deionized water for 5 times before being dried at 60 °C overnight. For comparison, the DP-modified TiO2 was prepared following the same procedure as above, except that HAuCl4·3H2O solution was not added in the first step. A series of samples were obtained by varying the stirring time (4–24 h). The prepared sample was ground into powder for use. It was named as TiO2(A)-X (A represents the anatase phase and X represents the time of treatment with the unit of hour).

    • The photocatalytic activity measurements on TiO2 were carried out by the degradation of MB solution using a 300 W xenon lamp (PLS-SXE-300, Beijing PerfectLight Technology Co., Ltd.). 5 mg of the prepared TiO2(A)-X was added to 50 mL of MB solution (0.02 mmol/L, pH≈7) in a reactor and sonicated for 2 min to get the homogeneous suspension. Prior to irradiation, the suspension was magnetically stirred for another 20 min in darkness in order to saturate the adsorption of MB. The temperature was kept at 20 °C by a coolant pump to reduce the thermal effect during the experiment. 2 mL suspension was taken out every 5 min. The catalysts in the suspensions were removed by centrifugation and the remained liquids were diluted and tested by a Shimadzu UV-3600 Spectrophotometer (Shimadzu, Japan) at λmax = 664 nm and a standard curve of absorbance vs. concentration of MB.

    • Since terephthalic acid (TPA) can react with ·OH and the production 2-hydroxy terephthalic acid (TPAOH) possesses unique fluorescence at around 423 nm with excitation of 324 nm [14, 15], we adopted this method to detect the presence of ·OH. The higher intensity of emission peak indicated that more ·OH was produced. 0.02 g NaOH was dissolved in 50 mL water, and 0.050 g TPA was subsequently put into the solution to sonicate in the dark to ensure the complete dissolution, and the pH of solution was adjusted to ~7 with hydrochloric acid. 5.0 mg of TiO2(A)-X was added into 50 mL of the prepared TPA solution. The solution was stirred in the dark for 20 min until the concentration of TPAOH remained unchanged. During UV light exposure, 2 mL suspension was taken out every 5 min. The catalysts in the suspensions were removed by centrifugation and the remained liquids were diluted and tested by F-4600 FL Spectrophotometer (Hitachi, Japan).

    • X-ray diffraction (XRD) patterns of catalysts were obtained with a Rigaku Smart Lab diffractometer (Rigaku Corporation, Tokyo, Japan) using Cu Kα radiation. The specific surface area and pore size distribution of the catalysts were analyzed using a surface area and porosity analyzer (Micromeritics Tristar II 3020M). Transmission electron microscopy (TEM) studies were carried out on a JEM-2011 microscope with field emission gun at 200 kV. Scanning electron microscopy (SEM) images of samples were obtained by a Hitachi 8220 electron microscope. The UV-Vis absorption of samples was recorded on a UV-Vis spectrometer (Shimadzu Solid 3700) using BaSO4 as a reference. The photoluminescence (PL) emission spectra were recorded under the excitation wavelength of 280 nm using a JY Fluorolog-3-Tou fluorescence spectrometer. The X-ray photoelectron spectra (XPS) were recorded on a Thermo ESCALAB250Xi spectrometer with an excitation source of monochromatized Al Kα (hν = 1486.6 eV) and a pass energy of 30 eV with the values of binding energies calibrated with the C 1s peak of contaminant carbon at 284.80 eV. The IR spectra for the samples were obtained using a Thermo Scientific Nicolet iS50 FT-IR Spectrometer with Harrick Praying Mantis cell at room temperature. The zeta potential analysis in deionized water was carried out using a Nanoparticle Size and Zeta Potential analyzer (Nanotrac Wave II) by electrophoresis method.

    III.   RESULTS AND DISCUSSION
    • FIG. 1(a) shows the photocatalytic performance of TiO2(A)-X and Au/TiO2(A)-17 on the degradation of MB in aqueous solution. To exclude the influence of the adsorption effect by TiO2 or Au/TiO2(A)-17 catalysts, the MB concentration was measured to be unchanged for at least 20 min in darkness before UV irradiation as shown in FIG. 1(a). The control experiment shows that ~20% MB in the solution without photocatalyst is eliminated after 30 min of UV irradiation. After adding TiO2(A)-0 (pristine commercial TiO2) to the MB solution, 57.8% of MB is eliminated. Compared with the TiO2(A)-0 sample, both the Au/TiO2 and modified TiO2 samples enhance the degradation rate of MB under UV irradiation. Unexpectedly, the TiO2(A)-17 sample shows an even higher photocatalytic performance than Au/TiO2(A)-17. In FIG. 1(a), the decay in concentration ratio (C/C0 is the ratio of the MB concentration at certain time to the MB concentration at 0 min) with the illumination time can be fitted by a first-order exponential curve and the rate constants (k) can be determined from the fitting by assuming the first-order kinetics of the photodegradation of MB. FIG. 1(b) shows the histogram of the k of TiO2 and Au/TiO2(A)-17 samples. The rate constant of TiO2(A)-17 is ~5 times as high as that of the pristine sample and ~1.5 times higher than that of Au/TiO2(A)-17. The photocatalytic activities for all the TiO2 remain unchanged after annealing at 400 °C in air for 4 h (FIG. S1 in Supplementary materials, SM).

      It is well known that during the heterogeneous photocatalytic processes electron-hole pairs are produced by the absorption of photons by semiconductors and subsequently redox reactions occur by the reactions between the excited e− and h+ with the reactants producing intermediates and then products [16, 17]. Identifying the roles of e−, h+, and intermediate species is essential to understand the enhanced photocatalytic performance of the degradation of MB on the DP-modified TiO2 photocatalysts.

      In order to assess the role of h+ and e− in photocatalytic reactions, ethylenediaminetetraacetic acid (EDTA) and KBrO3 are used respectively as hole and electron scavengers to quench h+ and e− in this work [18-20]. As shown in FIG. 1(c), the addition of 0.8 mmol/L EDTA (hole scavenger) considerably depresses the photocatalytic degradation rates of MB and all the rate constants k of TiO2 samples essentially drop to the same values. As opposed to that, the addition of 0.8 mmol/L KBrO3 (electron scavenger) enhances the photocatalytic degradation rates of MB and all the rate constants k increase while the trend of k plot with the TiO2 samples does not change. The control experiment in FIG. S2 (SM) excludes the direct oxidation of MB by KBrO3. These results clearly indicate that h+ plays important roles in the photodegradation of MB by TiO2(A). The hole scavenger (EDTA) decreases the surface h+ concentration and thus decreases the photodegradation rate of MB. The electron scavenger (KBrO3) decreases the surface e− concentration while increasing the surface h+ concentration due to the suppression of electron-hole recombination and thus increases the photodegradation rate of MB.

      The h+ lifetime is substantially shorter than the e−, and it has often been reported that oxygen species can couple to h+ on the photocatalyst surfaces forming hydroxyl radicals (·OH) to increase the use of h+ [6, 21]. The ·OH can effectively oxidize and degrade organic pollutants in water and is regarded as one of the most effective intermediates during the photodegradation processes [22]. To confirm the involvement of ·OH during the photodegradation of MB in this work, we use a typical ·OH eliminator (isopropyl alcohol, IPA) which can react rapidly with ·OH and interrupt the ·OH-mediated free radical chain reactions [16]. FIG. 1(d) shows that the presence of IPA notably inhibits the degradation of MB, and the extent of the inhibition increases with the concentration of IPA. Therefore, it can be concluded that ·OH is the primary intermediated species in the photocatalytic degradation reaction of MB by TiO2.

      The ·OH can be detected by employing TPA to generate the fluorescent product. It has been reported that TPA can react with ·OH to form TPAOH. The TPAOH shows characteristic fluorescence peak at 423 nm and can be used as a probe for ·OH [16, 23, 24]. As shown in FIG. 2(a) and FIG. S3 (in SM), no characteristic peak can be observed in the fluorescence spectra of the TPA solution with the TiO2 samples in dark. After UV irradiation, a typical peak of TPAOH appears and the peak intensity increases with the irradiation time. FIG. 2(a) shows that TiO2(A)-17 generates the most amount of ·OH under the same conditions. This is in consistence with the experimental results observed in FIG. 1.

      It should be mentioned that ·OH can also be produced by a multi-step reaction of e− with O2 in solution as being suggested by many researchers [22, 25]. In FIG. 2(b), the addition of either EDTA or IPA significantly decreases the ·OH (TPAOH) concentration. This clearly indicates that ·OH species is mainly produced from h+ in this experiment.

    • To further investigate the origin of the enhanced photocatalytic performance of the modified TiO2 by the DP treatment, detailed characterizations of the series of 5 TiO2 samples have been performed. The XRD patterns of the 5 TiO2 samples in FIG. S4 (SM) show that the DP treatment did not change the crystalline structure of anatase TiO2 (JCPDS No. 21-1272). TEM and SEM images (FIG. S5 in SM) also show that the size (~20 nm) and shape of TiO2 nanoparticles do not change after the DP treatment. The UV-Vis diffuse reflectance spectra in FIG. S6 (SM) exhibit a typical absorption in the UV region of the TiO2 samples and no significant changes of the optical absorption and the band gap of TiO2 after the DP treatment can be found.

      The N2 adsorption/desorption isothermal curves of the TiO2 are shown in FIG. S7 (SM). All the isotherms in FIG. S7 (SM) are of type IV with the H3 hysteresis loop according to IUPAC classification [26]. The type H3 hysteresis loop may be caused by the existence of non-rigid aggregates of particles or the assemblages of slit-shaped pores [27]. The average pore size was obtained from the maximum of pore size distribution curves for all the synthesized samples using BJH method (inset in FIG. S7 (SM)). The treatment of TiO2 by DP method slightly decreases the average pore size from ~10 nm to ~8 nm. Table S1 (SM) shows the values of BET specific surface area, pore volume and pore diameter of the pristine and modified TiO2 samples. The specific surface area of TiO2(A)-17 catalyst (169 m2/g) is 1.4 times the specific area of TiO2(A)-0 (122 m2/g). Therefore, the 5 times increase of the photocatalytic efficiency of TiO2(A)-17 than TiO2(A)-0 is not mainly caused by the increase of the specific surface area.

      The XPS of the 5 TiO2 samples was measured and the survey XPS spectra show the presence of Ti, O, and C elements (FIG. S8 in SM). FIG. 3(a) shows the Ti 2p spectra of the 5 TiO2 sample. The peaks of Ti 2p3/2 at 458.6 eV and 2p1/2 at 464.3 eV with symmetric shapes indicate that Ti has a chemical valence of Ti4+. The O 1s peak can be deconvoluted into 3 peaks at 529.8 eV, 530.9 eV, and 532.7 eV (FIG. 3(b)). The 529.8 eV peak with the full width at half maximum (FWHM) of 1.2 eV is from the lattice O of TiO2 [28]. The 530.9 eV peak with the FWHM of 1.6 eV is from the hydroxyl species (${\rm{OH}}_{\rm{ad}}^- $) on TiO2 [29]. The broad FWHM indicates the presence of versatile chemical environment for ${\rm{OH}}_{\rm{ad}}^- $ on TiO2 particles and the interaction between ${\rm{OH}}_{\rm{ad}}^- $ and adsorbed H2O. The 532.7 eV is ascribed to the adsorbed H2O [21]. The ratios of the integrated peak areas of the three O 1s peaks of 5 TiO2 samples are listed in Table S2 (SM). It shows that the amount of ${\rm{OH}}_{\rm{ad}}^- $ significantly increases by the DP treatment, and TiO2(A)-17 has a significantly higher number of OH− groups and adsorbed H2O than the other samples.

      The presence of ${\rm{OH}}_{\rm{ad}}^- $ and adsorbed H2O was further evidenced by IR analysis. Two absorption bands at 3000–3630 and 3660–3750 cm−1 are observed (FIG. 3(c)). The 3000–3630 cm−1 band is assigned to hydrogen-bonded OH stretching, and the 3660–3750 cm−1 band is assigned to the free OH stretching band from the isolated ${\rm{OH}}_{\rm{ad}}^- $ and/or adsorbed H2O that are not involved in hydrogen bonding [6]. The strongest absorption of the above two bands at TiO2(A)-17 sample also indicates the highest population of the ${\rm{OH}}_{\rm{ad}}^- $ and adsorbed H2O.

      The influence by the presence of OH−ad and adsorbed H2O was further investigated by the zeta potential and PL measurements. The zeta potentials of TiO2 in FIG. 4(a) indicate that the surface charge of TiO2 changes from the positive to the negative after the DP treatment due to the increase of surface ${\rm{OH}}_{\rm{ad}}^- $ groups. TiO2(A)-17 has the most negative zeta potential (0.6 mV), i.e., it has the most abundant surface ${\rm{OH}}_{\rm{ad}}^- $ groups. Thus, as a form of cationic dye, MB prefers to be electrostatically attracted by TiO2(A)-17 than other samples.

      FIG. 4(b) shows the PL spectra of 5 TiO2 samples. A broad emission peak at ~450 nm is due to the trap-assisted recombination of the photoexcited e− and h+ [30]. Compared with other samples, the PL peak intensity is significantly lower on TiO2(A)-17. In other word, the recombination of the electron-hole is depressed on TiO2(A)-17, which can be ascribed to the presence of surface ${\rm{OH}}_{\rm{ad}}^- $ groups. The elongated photogenerated carrier lifetime caused by the hydrogen bonding between surface ${\rm{OH}}_{\rm{ad}}^- $ and H2O on anatase TiO2 nanoparticles has been reported by K. Shirai et al. using water-coverage-controlled steady and transient infrared absorption spectroscopy and ab initio calculations [6].

    • Therefore, the mechanism of the enhanced photocatalytic performance of MB degradation on TiO2(A)-17 by DP treatment is proposed in FIG. 5. The TiO2 surface with more ${\rm{OH}}_{\rm{ad}}^- $ and H2O species by DP treatment facilitates the production of ·OH formed by the reaction with photoexcited h+, and the increase of formed ·OH accelerates the photodegradation rate of MB.

    IV.   CONCLUSION
    • In conclusion, we found that the DP method frequently used for synthesizing supported metal catalysts can significantly change the catalytic properties of support itself.

      (i) A series of TiO2 samples prepared with different time of DP treatment without Au loading showed variable photocatalytic performances towards MB degradation.

      (ii) Using electron and hole scavengers and fluorescence probe detection method, ·OH generated by photoexcited h+ is identified as the main intermediate reactive species during the degradation reaction.

      (iii) XPS and IR spectra show that TiO2(A)-17 after DP treatment has the most amount of surface ${\rm{OH}}_{\rm{ad}}^- $ species. The presence of surface ${\rm{OH}}_{\rm{ad}}^- $ species not only changes the surface zeta potential favoring the attraction of cationic MB, but also depresses the electron-hole recombination and enhances the photodegradation rate of MB by hole-produced ·OH.

      These results reveal the role of the ${\rm{OH}}_{\rm{ad}}^- $ caused by the DP methods on the photocatalytic reactions, and remind us to be cautious about the change of the support properties while preparing supported metal catalysts using DP methods.

      Supplementary materials: The MB photodegradation rate constants (k) of TiO2 catalysts before and after calcination at 400 °C in air for 4 h; fluorescence spectra, XRD patterns, TEM and SEM micrographs, UV-Vis absorption spectra, N2 adsorption-desorption isotherms, pore size distribution curves, XPS survey spectra of TiO2 samples; BET surface area, the pore volumes and pore diameters of the TiO2 powders, the ratios of the integrated peak areas of lattice O, ${\rm{OH}}_{\rm{ad}}^- $ and H2Oad are shown.