Gold nanoclusters (AuNCs) composed of tens to hundreds of atoms with a core size of 1–2 nm are a new class of nanomaterials gaining significant research interest because of their excellent optical properties [1, 2]. Due to the small size of AuNCs, they possess discrete orbitals which lead to their strong and tunable fluorescence properties [3, 4]. AuNCs have been recognized as fluorescent material under one-photon excitation [5−7] and they also show nonlinear optical properties [8−10]. For example, it has been demonstrated that quantum-size AuNCs have outstanding two-photon absorption, which makes them suitable for two-photon fluorescence (TPF) bio-imaging applications [11−15]. This is important because TPF is known to have the advantages of deeper penetration into the tissues, reduced sample photodamage, and diminished auto-fluorescence [16, 17]. TPF was also demonstrated to be a powerful technique that can be applied to investigate the photocatalytic activities, surfaces and interfacial changes, and surface defects of fluorescence nanomaterials [11, 18−24]. The TPF signals were observed to be very sensitive to the smallest environmental, structural, and surface photocatalytic changes of the target nanomaterials [18−20, 24].
It has been revealed that photocatalytic reactions occurring on the surface of AuNCs notably influence their fluorescence properties [13, 25, 26]. Tailoring the surface charges and capping ligand play a key role in modifying the optical and electric properties of AuNCs by changing their band gaps and photocatalysis capabilities [25]. Several experimental studies have addressed the photocatalytic properties of different atomically precise AuNCs [12, 25, 27, 28]. When the number of gold atoms in the AuNCs decreases, their band gap increases [29−31], affecting their excited state properties, such as excitation energy, lifetime, and fluorescence. Wu and Jin showed that capping ligands impacted the photoluminescence efficiency of the thiolate-protected AuNCs [32]. Additionally, Li et al. attributed the higher catalytic activities of AuNCs to the less bulky ligand [33]. Thus, band gap and capping ligand modification strongly affect the photocatalytic redox reactivities of the nanoclusters [34−38].
In this work, we synthesized two water-soluble gold clusters protected with captopril (Capt) and glutathione (GSH), namely, Au25(Capt)18 and Au15(GSH)13, and investigated their fluorescence efficiencies which are closely related to the photocatalytic oxidation of the gold atoms. It was found that upon irradiation of femtosecond near-infrared (NIR) laser with 810 nm wavelength, the TPF emission of Au25(Capt)18 with a smaller band gap (~1.36 eV) decayed with time, indicating the occurrence of photocatalytic oxidation on the cluster surface. On the other hand, the TPF emission from Au15(GSH)13 with a larger band gap (~2.57 eV) was stable upon the same excitation. One-photon excitation fluorescence measurements with photon energies beyond the two band gaps showed a decay in the fluorescence emissions from both AuNCs, confirming the interpretation of photocatalytic oxidation induced fluorescence decay. This comparison also shows another advantage of the two-photon excitation fluorescence, i.e., the application of photon with less energy avoids the occurrence of photocatalytic oxidation, thus leading to stable fluorescence emission. Furthermore, the photo-induced oxidation and reduction processes on the surface of Au25(Capt)18 were analyzed upon irradiation with the NIR laser light and introducing of various agents (N2, dopamine, H2O2, HNO3).
-
Hydrogen tetrachloroaurate (III) (HAuCl4-3H2O, 99.99%) was purchased from Alfa Aesar (Shanghai, China) Chemicals Co., Ltd. Tetraethylammonium bromide (TOABr, 99%) and potassium bromide (KBr, 99%) were purchased from Energy Chemical Co., Ltd. (Shanghai, China). Sodium hydroxide (NaOH, 99.99%) was purchased from Sigma-Aldrich (Shanghai, China). Captopril (Capt, 99%) was purchased from BiDe Pharmaceutical Technology Co., Ltd (Shanghai, China). L-glutathione reduced (L-GSH, 99%) was purchased from Aladdin (Shanghai, China). Isopropanol ((CH3)2CHOH, ≥ 99.7%), methanol (MeOH, 99%), and ethanol (EtOH, 99%) were purchased from Xilong Scientific (Guangdong, China). Sodium borohydride (NaBH4, ≥ 97.0%) was purchased from Ling Feng Chemical Reagent Co., Ltd. (Shanghai, China). Hydrogen peroxide (H2O2, mass fraction 30%, AR) was purchased from Donghong Industrial Development Co., Ltd (Guangzhou, China). Nitric acid (HNO3, mass fraction 65%–68%, GR) was purchased from Huachengda Chemical Co., Ltd. (Zhuhai, China). Nitrogen (N2, 99.999%) was purchased from Xiangyuan Industrial Gas Co., Ltd. (Guangzhou, China). Deionized water (18.2 MΩ·cm) was obtained from a water purification system (WP-UP-UV-20, Sichuan Water Technology Development Co., Ltd., Chengdu, China). All reagents were used as received.
-
Au25(Capt)18 clusters were synthesized using the method applied in a previous literature [39] and shown schematically in Scheme S1 in Supplementary materials (SM). First, HAuCl4·3H2O (0.20 mmol) and TOABr (0.23 mmol) were dissolved in 10 mL of methanol and stirred vigorously. The color of the mixture changed from yellow-orange to dark red. 20 min later, captopril (2 mmol, dissolved in 5 mL of methanol) was quickly injected into the mixed solution with stirring. The color of the solution rapidly changed to white. After 30 min, NaBH4 (2 mmol, in 5 mL of cold water) was quickly added to the mixture with fast stirring. The color of the solution immediately changed to brownish black. The stirring was continued for 8 h. Then, the solution was centrifuged to remove insoluble, unreacted Au(I):thiolate polymer residuals [39], which are undesired intermediate products and do not participate in the formation of gold nanoclusters. The centrifugated solution (supernatant) was collected and concentrated using the rotary evaporation method. Then, ethanol was added to the solution to precipitate the clusters. The precipitate was then washed several times using 3–4 mL of methanol to get a dispersion of Au25(Capt)18 in ~10 mL methanol. Finally, ~30 mL of ethanol was added in the dispersion to get the Au25(Capt)18 precipitation and then dried under vacuum condition.
Au15(GSH)13 clusters were prepared as shown schematically in Scheme S2 (SM) which follows the method previously reported in Ref.[40] with minor changes, i.e., the highly toxic acetonitrile solvent was replaced by isopropanol, both of which have similar polarity and can both precipitate gold nanoclusters. First, the freshly prepared aqueous solutions of HAuCl4 (4 mmol/L, 10 mL) and L-GSH (6 mmol/L, 10 mL) were mixed and stirred vigorously for 6.5 h at 90 °C. The synthesized clusters were precipitated by adding 60 mL isopropanol to the solution. Then, the solution was centrifuged at 10000 r/min for 10 min to discard the supernatant. The residues with clusters were washed for three times using a mixture of deionized water and isopropanol (1:3 volume ratio). The purified clusters were dried under vacuum for 12 h and stored in a refrigerator at 4 °C.
-
The absorption spectra of the AuNCs were measured using a spectrophotometer (Shimadzu UV-1800, Suzhou, China). During the experiment, the aqueous solution of AuNCs was placed in a cleaned quartz cuvette (~1 cm). One-photon fluorescence spectra of the AuNCs in the aqueous solution were tested in a 1 cm four-way quartz cuvette using a fluorescence spectrophotometer (F-7000, Hitachi, Japan). The FTIR spectra of Au25(Capt)18 and Au15(GSH)13 in solid state were tested using an FTIR spectrometer (Nicolet iS50, Thermo Fisher). The emission spectra from the AuNCs under the NIR excitation were recorded with the setup as reported previously [18, 41] and shown in Scheme S3. Briefly, a Ti:sapphire laser (MaiTai-HP, Spectra-Physics) at the wavelength of 810 nm was employed as the excitation light. After passing through a long pass filter (FGL9, > 720 nm), the light beam with a pulse width of about 100 fs and a repetition of 80 MHz was focused on the target AuNCs solution under stirring in a cylindrical quartz cell with inner diameter of ~13 mm. The emitted signal was passed through a band pass filter (FGB37S, 335–610 nm, Thorlabs) and directed toward the monochromator (Omni-λ1509, Zolix Instruments Co., Ltd, China) for spectra analysis. A PMT (Hamamatsu R-1527p, −900 V) was used to collect the signal at different wavelengths and a photon counter (SR400, Stanford Research System) was used to recorded the output signals from the PMTs after they were 5 times amplified by a preamplifier (SR445A, Stanford Research System). Finally, a computer recorded the photon counts. During the experiment, the PMT was kept at the voltage of −900 V. The laboratory temperature and humidity were controlled at 21±1 °C and 40%±5%, respectively. The sample temperature inside the quartz cell was tuned by a heater (Songdao Heating Sensor Co., Ltd., Shanghai, China) and monitored with a digital thermometer (D5770-01-1EA, Aladdin Biochemical Technology Co., Ltd., Shanghai, China).
-
The TEM images of the two AuNCs were measured using a JEM-3200FS electron microscope (EM-3200FS, JEOL, Japan). The gold cluster samples were sonicated in an ultrasonic machine (KQ-300DE, 40 kHz, 300 W, Kunshan Ultrasonic Instrument Co., Ltd., Kunshan, China) for 30 min. Then, 5 µL of the sample was drop casted on a carbon-coated copper grid and dried for 15 min at room temperature before the TEM imaging.
-
FIG. 1(a) displays the UV-Vis spectrum of Au25(Capt)18. The absorption peaks at about 670 nm and 780 nm correspond to the HOMO to LUMO transitions (intraband (sp←sp) transition) [2, 42, 43]. It has an onset wavelength (λonset) of about 910 nm (optical band gap Eg ~1.36 eV) [42, 44−46]. The absorption peak at about 450 nm arises from the interband (sp←d) transition. FIG. 1(b) shows the UV-Vis spectrum of Au15(GSH)13. The absorption spectrum monotonically increases as the wavelength decreases with a shoulder peak of about 400 nm and an onset wavelength of about 480 nm (Eg ~2.57 eV). The strong absorption arises from mixed interband (sp←d) and intraband (sp←sp) transitions [47, 48]. FIG. 1(c) indicates the schematic view of intraband and interband transitions for the gold clusters [49]. The absorption features of both AuNCs resemble the absorption of Au25(Capt)18 and Au15(GSH)13 reported previously [27, 34, 39, 40, 50, 51].
Fourier transform infrared spectra (FTIR) measurements with Capt, Au25(Capt)18, GSH, and Au15(GSH)13 in the solid state were performed and are shown in FIG. 2. The spectra indicate the disappearance of the S–H stretching vibrational mode in the range of 2550–2600 cm−l in Au25(Capt)18 and Au15(GSH)13, representing the cleavage of S–H bond as well as the binding of Capt/GSH ligand onto the surface of Au25(Capt)18/Au15(GSH)13 via Au–S bonding. FIG. 2 also shows that the stretching vibrational mode C=O of the free carboxylic acid group (~1735 cm−1) in ligand Capt/GSH disappeared or weakened in the formation of gold cluster because of their interaction with the gold surface due to their strong electron donating properties [32]. The FTIR spectra analysis also matched well with previous results of the AuNCs materials [32, 34, 52].
The morphologies of the two AuNCs were investigated by TEM with the results shown in FIG. 3 (a–d). The size distribution plot of the clusters was obtained from the images as shown in FIG. 4 (a, b). The mean size values of the gold clusters were obtained as 2.17±0.39 nm for Au25(Capt)18 and 2.16±0.44 nm for Au15(GSH)13, respectively.
Fluorescence emission spectra of Au25(Capt)18 and Au15(GSH)13 were investigated by single photon excitation as shown in FIG. 5. For Au25(Capt)18, a broad emission centered at ~725 nm was observed with an excitation wavelength of 514 nm. For Au15(GSH)13, a broad emission centered at ~605 nm was observed with an excitation wavelength of 370 nm. These spectra are also similar to those reported before [39, 40].
-
The nonlinear optical scattering including second harmonic generation (SHG) and TPF have been shown to provide valuable information on the surface structure, dynamics, and photocatalytic redox reactions on nanomaterials [47, 48, 53−57]. Therefore, we used 810 nm femtosecond laser (300 mW) to excite the prepared AuNCs and analyzed the emission spectra (FIG. 6). As shown in FIG. 6(a), the emission spectrum of Au25(Capt)18 was mainly composed of two peaks, a relatively strong broad peak centered at ~500 nm and a weak shoulder peak at ~405 nm. The small peak at 405 nm can be attributed to the hyper-Rayleigh scattering from the water molecules and a weak SHG contribution from the gold cluster as reported previously [58]. The broad peak at ~500 nm was attributable to the TPF emission due to the metal-ligand and ligand-metal-metal charge transfer excitation [48, 55, 56]. The emission from Au15(GSH)13 was mainly composed of three peaks (FIG. 6(c)). A separated weak peak at ~405 nm can be attributed to the hyper-Rayleigh scattering of water and the weak SHG contribution from the gold cluster. A weak broad peak centered at 450 nm is attributable to the metal-metal transition, and the relatively strong broad peak centered at ~565 nm is attributable to the ligand-metal and ligand-metal-metal charge transfer excitations [56].
In the experiments, the TPF spectrum of Au25(Capt)18 decayed with continuous irradiation of the NIR laser (FIG. 6(b)). In contrast, the TPF spectra for the Au15(GSH)13 remained stable (FIG. 6(d)) upon the laser irradiation. To confirm that the decay of the TPF emission from Au25(Capt)18 was caused by the irradiation of NIR laser, experiments were carried out with some of the laser pulses intentionally blocked and the result was shown in FIG. 6(b). As expected, the decay of the TPF intensity was notably weakened, confirming it a laser induced effect. The decrease of the TPF emission from the surface of silver particles has been explained with the photo-oxidation of the silver atom on the surface [18, 24, 59, 60]. However, gold nanoparticles with diameters as tens of nanometers were observed to have stable TPF emission upon irradiation of the NIR laser, indicating that surface gold in the nanoparticles are hard to be influenced by photo-oxidation [19]. Here, the decay of the TPF emission from Au25(Capt)18 but not Au15(GSH)13 needs to be understood.
Nitrogen (N2) purging experiments were used to test if the decay of the TPF emission from Au25(Capt)18 is related to the surface oxidization of gold atoms. It was known that TPF and SHG signals of the silver or gold nanoparticles could be modified due to the alteration of redox properties of their corresponding surfaces with laser irradiation and/or redox agents [61, 62]. For example, by adding NaBH4 to the colloidal solution of silver or gold nanoparticles, BH4− donates electrons to the metal particles and increases the surface non-linearity as well the efficiency of electron-hole recombination, leading to enhanced SHG and TPF signals [18]. Similarly, purging nitrogen to the colloidal solution of silver nanoparticles avoids the exposure of silver nanoparticles surfaces to O2 and provides them stability under laser light irradiation [18, 19]. In FIG. 7(a), the TPF remains stable upon the irradiation of NIR laser with continuous purging of nitrogen (N2), confirming the role of oxygen on the surface process that resulted in the TPF decay. The requirement of both laser irradiation and oxygen points to the photo-catalytic oxidization process of the surface gold atoms. In FIG. 7(b), Au25(Capt)18 was firstly irradiated with the NIR laser without N2 purging, then N2 purging was introduced in the time range of ~2037–2700 s, which shows a recovery of the TPF emission from the photo-catalytic reduction of the gold clusters.
It has been reported that Au25(Capt)18 cluster was synthetized with a negative charge, i.e., [Au25(Capt)18]− [39, 58]. According to a previous literature, the negative charge of [Au25(Capt)18]− transferred to the higher charge states due to thermal radiation [39], resulting in damping in their UV-Vis peak. Other literatures also showed that neutral and higher charge states of [Au25(SC2H4Ph)18]− and [Au25(SG)18]− were obtained due to air oxidation [32, 42, 63], which also shows a similar decrease in their UV-Vis spectra. In our experiments, the decay of the TPF emission from Au25(Capt)18 is accompanied by a decrease in its absorption spectrum (FIG. 8), which is similar to the observation of a decreased absorbance of Au25(Capt)18 when it is exposed to thermal irradiation [39]. Therefore, it is reasonable to believe that the TPF decay is also induced by the same photo-oxidation mechanism, with the converting of [Au25(Capt)18]− to Au25(Capt)18. At the same time, the recovery of the TPF emission with N2 purging also indicates that photo-oxidation can be partly reversed by the NIR irradiation with the oxygen excluded.
The reason that the photo-catalytic oxidization influenced Au25(Capt)18 but not Au15(GSH)13 can be interpreted by the different band gaps of the two AuNCs. As aforementioned, the band gap of Au25(Capt)18 (~1.36 eV) is smaller than the band gap of Au15(GSH)13 (~2.57 eV). Therefore, Au25(Capt)18 can be easily excited to the higher energy states by NIR laser with photon energy as 1.53 eV in the presence of O2. For Au15(GSH)13, although two-photon excitation provides TPF emission from the gold clusters, the energy of the exciting photon is insufficient to induce a detectable photo-catalytic oxidization.
To support this interpretation, we tested the stability of one photon fluorescence with the photon energy of the excitation light beyond the band gaps of the AuNCs. In this experiment, Au25(Capt)18 and Au15(GSH)13 were continuously irradiated with light at 514 nm (photon energy 2.41 eV , which is beyond ~1.36 eV) and 370 nm (photon energy 3.35 eV , which is beyond ~2.57 eV), respectively. As shown in FIG. 9 (a, b), the fluorescence intensities decrease for both samples, showing the photo-catalytic oxidization for both AuNCs. Therefore, this comparison between the one photon fluorescence and TPF reflects the advantage of TPF excitation, i.e., the excitation with laser at a relatively long wavelength can avoid the photo-oxidization of some AuNCs, providing stable fluorescence emission for the bioimaging or sensing applications. Cover of AuNCs also influences TPF stability, the different capping ligands may cause different photo-oxidation behavior, as suggested by a previous report [27]. In contrast to captopril in Au25(Capt)18, the capping ligand glutathione in Au15(GSH)13 is bulky and the percentage of their capping to the gold atoms is comparatively higher, which covers more surface area of the gold clusters and provides more electrons to the gold atoms to keep them stable and vice versa.
To test the stability of the influence of surface ligand on the TPF from Au25(Capt)18, several ligands were added to the sample solution with the NIR irradiation (FIG. 10). Dopamine which is known to be able to transfer electron to metal [64] and two oxidizing agents (H2O2, HNO3) were used in the experiments. As shown in FIG. 10(b), the TPF signal degradation was weakened upon the addition of dopamine in the sample, indicating an electron transfer to Au25(Capt)18 which prevents the oxidation of the AuNCs. On contrary, the addition of H2O2 and HNO3 accelerated the decay of the TPF emission, indicating a promoted photo-oxidation process (FIG. 10(c, d)). The influence of ligands on the TPF stability also confirmed the effect of photo-catalytic redox on the fluorescence stability of Au25(Capt)18. At the same time, further investigations on the fluorescence stability of AuNCs with various surface modification are expected to provide more clues on how to obtain AuNCs with better fluorescent performance.
-
In summary, the effects of bandgap and capping ligand on the photo-oxidation and photo-stabilities of two water-soluble thiolate-based AuNCs under laser irradiation were investigated based on their one-photon and two-photon fluorescence emissions. It was shown that the TPF from Au25(Capt)18 with a relatively low optical bandgap (Eg≈1.36 eV) decreased upon the irradiation of NIR laser with a photon energy of 1.53 eV. The TPF decreasing was attributable to the photo-oxidation of the gold cluster. In contrast, Au15(GSH)13 with a large band gap (Eg≈2.57 eV) was not subject to the influence of photo-oxidization from the NIR laser and emitted stable TPF signals. One photon excitation with laser photon energies of 2.41 eV and 3.35 eV were used to test the stability of fluorescence from Au25(Capt)18 and Au15(GSH)13, respectively. It was observed as expected that the fluorescence from both gold clusters decayed with the irradiation of laser with relatively large photon energy. Several redox ligands were also introduced to influence the photo-oxidization on the surface of Au25(Capt)18 and its TPF stability. Based on these observations, this work provides information on the relationship between the fluorescence from gold clusters and the photo-catalytic redox of at their surface.
Supplementary materials: Schematic diagrams of the synthesis of gold clusters and the experimental setup for the emission spectra analysis are shown.
Stability of Fluorescence Emission from Gold Nanoclusters and Photocatalytic Redox on Surface†
- Received Date: 16/12/2023
- Available Online: 27/06/2024
-
Key words:
- Gold nanoclusters /
- Band gap /
- Two-photon fluorescence /
- Photocatalytic redox
Abstract: The fluorescent emission and the photocatalytic activity of gold nanoclusters (AuNCs) are important properties of AuNCs. Here, we synthesized water-soluble, captopril (Capt) and glutathione (GSH) covered Au25(Capt)18 and Au15(GSH)13 nanoclusters and investigated their fluorescence stabilities which are correlated with the photo-redox of their surface. It was observed that Au25(Capt)18 exhibited a decay in its two-photon fluorescence emission induced by surface oxidation upon irradiation of femtosecond near-infrared laser (810 nm, 300 mW) in the presence of oxygen (O2). On the other hand, the two-photon fluorescence from Au15(GSH)13 was stable upon the same excitation. The different stabilities of the fluorescence of the two AuNCs were attributed to their different band gaps. This interpretation was confirmed by one-photon excitation with photon energy beyond the band gaps of the two AuNCs. Using experiments with the addition of several agents, the photocatalytic redox activities of gold atoms on the surface of Au25(Capt)18 were understood and tuned.