With the rapid consumption of non-renewable fossil resources and the growing demand for green chemicals in the development of human society, the utilization of renewable biomass resources has attracted widespread research. Many catalytic systems up to now, could realize the production of high value-added chemicals or fuel alternatives from various biomass feedstocks [1−3]. Among more than 300 kinds of biomass-based chemicals, levulinic acid was one of the most significant biomass platform chemicals [4, 5]. Levulinic acid could be produced from the acid catalyzed hydrolysis of biomass containing pentose, hexose or furfuryl alcohol, and could be further converted to a series of high value-added chemicals, such as γ-valerolactone, levulinate esters, angelica lactone, methyl tetrahydrofuran, or 1,4-pentanediol. Among them, γ-valerolactone was considered as an important building block. It could be used in the synthesis of pharmaceuticals, perfumes, nylon materials and jet fuel, or used directly as edible flavor improver, fuel additive or green solvent [6−8].
The conversion of levulinic acid to γ-valerolactone was studied in various catalytic systems using different metals, such as Ru [9−19], Pd [20−22], Ir [23−25], Pt [26, 27], Ni [28−34], Cu [35, 36], Co [37−42] or bimetallic catalysts [43−51]. Among these catalysts, Ru has a special ability for the hydrogenation of carbonyl group and performed better than other noble or non-noble metals [52]. For example, Molleti et al. used Ru/OMS-2 with moderate acidic sites and well dispersed Ru as catalyst, and reached 99.9% yield of γ-valerolactone at 100 °C and 3 MPa [9]. Koley et al. used Ru exchanged tungstophosphoric acid catalyst and realized the full conversion of levulinic acid to γ-valerolactone at 130 °C and 1 MPa [10]. Sorokina et al. reported the Ru nanoparticle containing nanocomposites based on hyperbranched pyridylphenylene polymer and got nearly quantitative yield of γ-valerolactone at 100 °C and 2 MPa [11]. The higher dispersity of Ru played a significant role in this reaction and some single atomic catalysts were reported. Han et al. prepared atomically dispersed Ru anchored on uniform subsupporter WOx clusters on carbon–nitrogen. It could reach over 99% conversion of levulinic acid and nearly 100% selectivity of γ-valerolactone at 100 °C and 2 MPa in solvent-free condition [12]. Zhang et al. prepared single Ru atoms on a TiO2@nitrogen doped porous carbon support catalyst and could reach as high as 278 molGVL·molRu−1h−1 at 30 °C and 6 MPa [13]. Yang et al. reported Ru single atoms anchored on a one-dimensional carbon fiber@graphitic carbon nitride hierarchy. The excellent durability under harsh reaction conditions was due to the one-dimensional hierarchy which enhanced electron/mass transfer [14]. Carbon materials, with adjustable morphology, were another important support. Ruiz-Bernal et al. used commercial and biomass-derived activated carbons as the support of Ru catalyst, and found out that carbon with more acidic sites showed better catalytic properties [15]. Wang et al. used carbon nanospheres support Ru nanoparticles with special C=O species on interface which had electronic metal-support interaction with Ru, and the electron-deficient Ru site improved the hydrogenation of levulinic acid [16]. Bounoukta et al. used Ru supported on functionalized carbon nanofibers to get full conversion of levulinic acid to γ-valerolactone at 140 °C and 1 MPa [17]. They also used cotton stalks-based biochars to support Ru and reached 95% conversion of levulinic acid and 92% yield of γ-valerolactone [18]. There were also some theoretical researches. Wei et al. developed a pore-scale multiphase reactive transport model based on the lattice Boltzmann method during the Ru/C catalyzed hydrogenation of levulinic acid to γ-valerolactone [19]. Although nearly equivalent production of γ-valerolactone from levulinic acid was achieved in the research works above, the reaction still needed to be proceeded under high hydrogen pressure. In our previous work, Pd was added to improve the activation of hydrogen at ambient conditions. The RuPd/TiO2 was employed at hydrogen pressure of as low as 15 kPa and performed well. However, the high price of Pd catalyst limited its application [43].
As a reaction with significant industrialization potential, it was necessary to develop a stable and easily prepared low-cost catalyst. Most well-refined catalysts were difficult to scale up, had high costs, and their stability was difficult to ensure. Moreover, previous researches always stayed at lab-scale reactions and barely any continuous production was reported. Biomass itself was a high-quality raw material for the large-scale preparation of carbon materials. The heteroatoms such as nitrogen originally present in biomass can also be utilized to further enhance the stability and activity of the catalyst.
In this work, biomass material was used to prepare nitrogen doped carbon. After the loading of Ru, the Ru/NC catalyst was employed in the solvent-free hydrogenation of levulinic acid under ambient hydrogen pressure. The calcination temperature was optimized to get Ru/NC-800 catalyst with the highest intrinsic TOF of 358 h−1. The apparent activation energy was determined by kinetic experiments to be 59.5±2.1 kJ/mol. Moreover, and more significantly, a continuous reaction was performed on a fixed-bed reactor to give a 620 g/day productivity of γ-valerolactone. This work provided a new potential route for the future commercial production of γ-valerolactone from levulinic acid.
-
Chitosan (BR, code 69047438), levulinic acid (AR), γ-valerolactone (AR) were purchased from Sinopharm Chemical Reagent Co., Ltd. RuCl3·xH2O with Ru content of 37% was purchased from Shaanxi Kaida Chemical Engineering Co., Ltd. Deionized water was purchased from Hangzhou Wahaha Group Co., Ltd. The gases (Ar, N2, H2, and NH3) were purchased from Nanjing Special Gas Factory Co., Ltd. All the above reagents were used without any pretreatment.
Teflon-lined hydrothermal reactors (HTG-50-SS2) and tubular furnace were provided by Anhui CHEMN Instruments Co., Ltd. Schlenk tube was purchased from Synthware Glass Instruments Co., Ltd. The fixed bed reactor was customized from Anhui CHEMN Instruments Co., Ltd.
-
The NC-T was prepared by calcination of chitosan in tubular furnace in NH3 flow for 3 h. T was the calcination temperature in degrees Celcius.
The loading of Ru was proceeded with a wet-impregnation method. 1 g of NC-T was dispersed in 70 mL of acetone. Then the RuCl3·xH2O-acetone solution was added to the above suspension dropwise. The mixture was stirred at 40 °C for 20 h and dried in a rotary vacuum evaporator. The precursor was reduced in 1/9 H2/N2 flow at 280 °C for 3 h. After cooling down in N2 flow, Ru/NC-T was prepared.
In this work, all the content of Ru was 2 wt% by inductively coupled plasma-atomic emission spectrometry (ICP-AES).
-
The powder X-ray diffraction (pXRD) patterns of the catalysts were measured by an X’pert (PANalytical) diffractometer, using Cu Kα radiation at 40 kV and 40 mA, 2θ in the range of 10°−70°.
The scanning electron microscopy (SEM) images were taken with a HITACHI-SU8220 scanning electron microscope.
The temperature programmed desorption of H2 (H2-TPD) was performed on an automatic chemical adsorption instrument (VDsorb 91i, Quzhou Vodo Instrument Co., Ltd.). The TCD temperature was set at 80 °C. The gas flow was 40 sccm. The catalyst was first pretreated at 300 °C in Ar flow. After cooling down to room temperature, it was treated with H2 for 1 h and then purged with Ar for 1 h. Then it was heated up to 800 °C under Ar flow. Calcination of dispersity of Ru: using the quantitative loop with volume V0=2.24 mL to get TCD signal with area of S0 (take the average value of 10 data). In the TPD test, the desorption peak area was S1. Therefore, the volume of desorbed H2 was V=V0×S1/S0, the molar amount of desorbed H2 was n=V/24.05 at room temperature. Assuming that each surface Ru absorbed one molecule hydrogen, the molar amount of surface Ru was also n. The total weight of Ru based on ICP was m. Then the dispersity of Ru was 101.07×n/m.
The TOF based on total Ru was calculated as:
The TOF based on surface Ru was calculated as:
-
Batch reactor: 2 g of levulinic acid and 100 mg of catalyst were added to a Schlenk tube with a hydrogen balloon. The reaction was proceeded with 1200 r/min stirring at set temperature for set time. After reaction, the Schlenk tube was cooled down in ice-water mixture. The liquid was diluted with methanol to be analyzed by Shimadzu Nexis 2030 gas chromatography. The solid was washed by water for the recycling test.
Fixed bed reactor: the catalyst was treated through compression molding with 300 bar and broke to irregular spherical particles between 40–60 meshes. 2 g of catalyst was filled into the fixed bed reactor. The leakage test of the reactor used 5 MPa of N2 followed by 5 MPa of H2. Then the hydrogen flow was set to 100 mL/min. The feed rate of levulinic acid was 0.05, 0.1, 0.2, and 0.5 mL/min, respectively. After 1 h of reaction, the down-stream product was collected and tested for the first data point. Then the reaction was tested for 36 h.
-
SEM was used to observe the surface morphology of nitrogen-doped carbon supports, as shown in FIG. 1(A−F). The nitrogen-doped carbon materials calcined at 300 °C had a relatively large blocky structure. The structure was tight and thick with barely no porous structure, leading to very low surface area (Table S1 in Supplementary materials, SM). With the increase of temperature, the particle size of nitrogen-doped carbon material became broken and the size decreased gradually. The nitrogen-doped carbon calcined at 500−700 °C all had lamellar structure with smooth surface. When the calcination temperature was further increased to 800 °C, obvious cracks and crushing on the surface of the nitrogen-doped carbon materials could be clearly observed, and some smaller particles also appeared. The nitrogen-doped carbon became completely broken irregular flake, block or granular nanoparticles with nonuniform surface topography after being calcined at 900 °C. The surface area of NC-800 was the highest among these samples. The severe graphitization at 900 °C could lead to the decrease of surface area.
XRD patterns in FIG. 1(G) show that there basically presented amorphous phase when calcined at relatively low temperature. The broad peak between 20° and 30° was the characteristic signal of (002) surface of amorphous carbon. It indicated the existence of partially ordered graphite layer structure in the carbon. The non-uniform interlayer spacing led to the broad peak. This peak blue-shifted to higher diffraction angle compared with other reported carbon characteristic peak. It indicated smaller interlayer spacing of localized graphite layer in this material. It was due to the relatively regular structure of chitosan and some crystallized chitosan would form more regular structure of carbon during pyrolysis. The original structure of chitosan was beneficial to the graphitization. With the increase of calcination temperature, this broad peak gradually became narrower and higher, and shifted towards a large angle. It indicated that higher calcination temperature would promote the formation of regular layer of carbon and the graphitization. After further raising the calcination temperature to 800 °C, a significant signal of (002) surface of graphite-carbon can be clearly observed. For nitrogen-doped carbon calcined at 900 °C, the diffraction peak of graphitic carbon was very obvious.
-
The catalysts were evaluated for their performance in the hydrogenation of levulinic acid at a temperature of 80 °C for a duration of 2 h, the results are shown in FIG. 2. In each experiment, γ-valerolactone was exclusively produced, with selectivity nearing 100%. The conversion and yield were 20% using the Ru/NC-300 catalyst. However, the conversion and yield were improved to the range of 45%−55% with catalysts where the Ru/NC had been calcined at temperatures between 500 and 700 °C. The Ru/NC-800 catalyst demonstrated the highest activity, whereas further elevation of the calcination temperature led to a notable decrease in catalytic efficacy. Considering the above SEM images and BET surface area, it became evident that the surface morphology of the carbon support played a crucial role. The nitrogen-doped carbon support calcined at 300 °C exhibited a comparatively large block-like structure with a relatively low surface area, making it less than ideal for its intended application. In contrast, the nitrogen-doped carbon supports calcined within the range of 500−700 °C all featured lamellar block structures characterized by smoother and flatter surfaces, although their surface area was found to be inferior to that of the nitrogen-doped carbon supports calcined at 800 °C. When the calcination temperature was raised to 900 °C, there was a potential for the carbon surface structure to be compromised. Consequently, the nitrogen-doped carbon support that had been calcined at 800 °C emerged as the optimal choice for the loading of Ru in this context.
To further study the dispersion of Ru on nitrogen-doped carbon with various calcination temperatures, H2-TPD was employed to calculate the dispersion of Ru and the TOF was calculated based on both total Ru content and surface Ru content, as shown in Table I.
The Ru/NC-800 catalyst had the highest Ru dispersion of 32% among these catalysts. Based on the experimental results, TOF based on total Ru and surface Ru were calculated. In order to reduce the effect of the concentration changes of reactant during the reaction, all TOF values were calculated using the data with conversion below 30%, where the conversion rate was basically linearly positive correlated with the reaction time, as shown in Table S2 (SM). The TOF based on the total amount of Ru represented the amount of γ-valerolactone that can be produced per mol of Ru per hour in the catalyst used, which was also known as the apparent TOF of the catalyst. It can be seen that Ru/NC-800 catalyst has the highest apparent TOF value, reaching 115 molGVL·
${\mathrm{mol}}_{\mathrm{Ru}}^{-1} $ h−1 (Entry 5, Table I).However, because Ru was not fully exposed to the surface, the Ru inside those nanoparticles did not actually play a direct catalytic role in the reaction. Therefore, TOF based on the amount of Ru on the surface was calculated to evaluate the intrinsic activity of the catalyst. TOF based on the amount of surface Ru refers to the amount of γ-valerolactone that can be produced per mol of surface Ru per hour, which was also known as the intrinsic TOF of the catalyst. It can be seen that unlike the large difference in apparent TOF, the difference in intrinsic TOF values was not that large. The intrinsic TOF values of Ru/NC-700 and Ru/NC-800 were similar, while the intrinsic TOF values of several other catalysts were relatively lower. The Ru/NC-800 catalyst has the highest intrinsic TOF of 358 molGVL·
${\rm mol}_{\rm Ru}^{-1}$ h−1) (Entry 5, Table I).Based on the above discussions, the Ru/NC-800 has the highest catalytic activity, dispersity of Ru, apparent TOF and intrinsic TOF, and is the optimized catalyst.
-
The kinetic study with Ru/NC-800 was then carried out. The curves corresponding to the conversion of levulinic acid as a function of reaction time in the range of 50−80 °C are presented in FIG. 3(A). At 50 °C, 60 °C, 70 °C, and 80 °C, conversions and selectivity of more than 99% were achieved after 20 h, 12 h, 6 h, and 3 h of conversion, respectively. The reaction progress was fast in the early stage, but the reaction rate decreased significantly with the decrease of levulinic acid concentration in the later stage. Taking the reaction at 80 °C as an example, 53% conversion was achieved after only 0.5 h, and 95% conversion can be reached after reaction for 2 h. In order to achieve a conversion of more than 99%, the reaction time needs to be further extended to 3 h. Taking the conversion of 50 °C as an example, the conversion can reach 89% after 10 h, while 96% and 99% conversion were reached after 15 h and 20 h, respectively. The reaction was simulated with first-order reaction kinetics, and the fitting degree was more than 99.95%, as shown in FIG. 3(B).
Since hydrogen is always supplied at constant pressure using balloon during the reaction, the concentration of hydrogen did not change throughout the reaction. Therefore, the reaction rate was only related to the concentration of levulinic acid, that is, to the conversion of the reaction. The reaction of levulinic acid hydrogenation catalyzed by Ru/NC-800 basically revealed the first-order kinetic process, and its kinetic equation is shown as follows:
where c was the concentration of feedstock at a certain time, c0 was the original concentration of levulinic acid, k was the first-order reaction rate constant, and t was the reaction time.
As can be seen from FIG. 3(B), the rate constant of the reaction approximately doubles for every 10 °C increase in the reaction temperature. The apparent activation energy was 59.5±2.1 kJ/mol according to the Arrhenius equation, as shown in FIG. 3(C).
-
The catalyst recyclability test in batch reactor was proceeded in the reaction condition without full conversion to reveal the stability of catalyst. The conversion and yield were both 53% at 80 °C for 30 min. After five runs of reaction, no deactivation was observed, indicating an ultra-stable catalyst performance, as shown in FIG. 4.
-
As discussed above, the Ru/NC-800 was very active and stable in the hydrogenation of levulinic acid to γ-valerolactone in batch reactor. It indicated this catalytic system had potential for industrial application. Therefore, a series of reactions were performed in fixed bed reactor with various weight hourly space velocity (WHSV) at various temperature, as shown in FIG. 5.
The Ru/NC-800 catalyst could continuously catalyze the conversion of levulinic acid to γ-valerolactone for 36 h at 50−80 °C, and achieved a conversion rate of 20%−99% with deactivation rate of less than 2% depending on the reaction temperature and feed flow rate. For the purpose of full conversion, 99% selectivity of γ-valerolactone and 80 g/day yield can be achieved at 80 °C, 1.7 h−1 WHSV; while for the highest productivity, a 76% selectivity of γ-valerolactone and a yield of 620 g/day can be achieved at 80 °C, 17 h−1 WHSV.
-
In this work, biomass-derived chitosan was used to prepare nitrogen doped carbon supported Ru catalyst. The Ru/NC catalyst was employed in the solvent-free hydrogenation of levulinic acid under ambient hydrogen pressure at 50−80 °C to reach full conversion. The calcination temperature was optimized to get Ru/NC-800 catalyst with highest TOF. The apparent activation energy was 59.5±2.1 kJ/mol according to kinetic experiments. Significantly, the catalyst was small-scaled tested in a fixed-bed reactor with 620 g/day productivity of γ-valerolactone for 36 h. This work provided the potential of future commercial production of γ-valerolactone from levulinic acid.
Supplementary materials: BET surface area and reaction data.
Hydrogenation of Levulinic Acid over Biomass-based Ru/NC Catalyst
- Received Date: 18/03/2024
- Available Online: 27/12/2025
-
Key words:
- Hydrogenations /
- Levulinic acid /
- Biomass /
- Ru/NC /
- Catalyst
Abstract: The conversion of levulinic acid to γ-valerolactone is one of the most important reactions from biomass platform molecule to value-added chemicals. Ru-based catalysts have shown high activity and selectivity in previous studies but always required complex synthetic method or harsh reaction conditions. In this work, biomass-derived chitosan was used to prepare nitrogen doped carbon. After the loading of Ru, the Ru/NC (NC: nitrogen-doped carbon) catalyst was employed in the solvent-free hydrogenation of levulinic acid under ambient hydrogen pressure at 50−80 °C to reach full conversion. The calcination temperature was optimized to get Ru/NC-800 catalyst with high intrinsic turnover frequency of 358 h−1. The apparent activation energy was studied by kinetic experiments. More significantly, the catalyst was small-scaled tested for 36 h in a fix-bed reactor with 620 g/day productivity of γ-valerolactone. The catalyst can be easily synthesized and have high activity and stability, underscoring the potential of future commercial production of γ-valerolactone from levulinic acid.
首页
登录
注册


DownLoad: