Understanding materials’ mechanical and dynamic properties during the tensile process is significant to materials science and condensed matter physics [1]. Oxide ceramics have excellent properties such as good chemical and thermal stability, high strength, and wear resistance, use in high-temperature oxidation environments for a long time, which make them very attractive in engineering applications [2−6]. Nevertheless, under external forces, most ceramic materials have little or no plastic deformation, so the failure of ceramics is often a brittle fracture [5−7], resulting in disastrous damage [8]. Therefore, a key issue in industrial applications is to improve the tensile properties of oxide ceramics. To solve this problem, ceramics are commonly combined with other materials, such as ceramic particles, metals, carbon nanotubes, graphene sheets, polymers, etc. to give full play to their excellent properties [4, 6, 9].
Among various reinforced materials, metal-ceramic composites possess the superior performance of metals and ceramics, providing not only toughness, plasticity, and strength, but also hardness, stability, and corrosion resistance [10−13]. Therefore, metal-ceramic composites are commonly used in energy and electronic devices, as well as in aerospace for their wave-absorbing properties [14−17]. FeCo alloy is a typical binary alloy, and Al2O3 ceramics are useful in the research, preparation, and application of metal-ceramic composites due to their mature preparation technology and low cost [16, 18, 19].
The study on the mechanical properties of Al2O3/FeCo can shed light on the applications of metal-ceramic composite materials in industry. Recently, some experiments and calculations have been devoted to investigating its catalytic, wave-absorbing, and magnetic properties. In terms of catalysis, a kind of Al2O3/FeCo catalyst is used for the growth of carbon nanotubes from the catalytic decomposition of methane, which improves the yield and purity of carbon nanotubes [20]. It can also promote the CO2 methanation reaction [21] and provide theoretical guidance for the rational design of efficient catalysts. First-principles calculations and electronic paramagnetic resonance (EPR) experiments have elucidated the electron transfer and catalytic mechanism of (γ-Al2O3)/FeCo catalyst [22], thereby promoting the development of a highly efficient catalyst. Another valuable application of Al2O3/FeCo is that Al2O3-coated FeCo nano-capsules microspheres can be used as absorbers of electromagnetic (EM) waves [23]. Al2O3/FeCo composite prepared by mechanochemical synthesis has a wide bandwidth and thin thickness, making it an ideal material for microwave absorption [24]. Further experimental studies on the magnetic properties of the Al2O3/FeCo composite reveal that the Al2O3/FeCo-multilayers with FeCo-layers below the thickness of 1.74 nm exhibit superparamagnetic behavior at room temperature, and by exceeding this critical thickness, the neighboring FeCo starts to coalesce, resulting in ferromagnetic behavior [25]. However, underlying mechanism behind the magnetic properties exhibited by the Al2O3/FeCo composite remains unknown.
Experimental works suggest magnetic field to be a means of effective regulation in controlling chemical reaction rates [26], spin polarization [27], and order-disorder transitions of hydrogen bonds [28]. Furthermore, the application of an external magnetic field may lead to an increase in the elastic modulus [29]. However, few theoretical computational studies have attempted to elucidate the effects of the external magnetic field on the structure and properties of these systems. Understanding of the role of the external magnetic field in molecular dynamics (MD) simulation is still in the stage of infancy, and introducing a magnetic field for this study is a challenging task. So far, only a small amount of works have used MD simulation to investigate the impact of the external magnetic field.
Our present work focuses on understanding the mechanical properties and kinetic properties in the equilibrium state of the Al2O3/FeCo interface, both with and without the external magnetic field. MD simulation has been widely employed in the study of large-scale materials while greatly saving experimental resources, and revealing the macroscopic behavior resulting from microscopic interactions [30]. To promote the design and application of metal-ceramic composites, it is necessary to clarify the mechanical properties and micro-dynamics mechanism of the Al2O3/FeCo composite based on our reliable MD simulation of FeCo alloy [31] and Fe [32] under an external magnetic field.
The purpose of this work is to investigate the mechanical properties and microscale structure of the Al2O3/FeCo interface by obtaining its Young’s modulus from the stress-strain curve during the uniaxial tensile process. While obtaining the mean square displacement (MSD), diffusion coefficient, and radial distribution function (RDF) from MD trajectories, our simulations consider both with and without magnetism for the Fe and Co atoms. And then we investigate the impact of atomic magnetism and the external magnetic field on the interface. Overall, this study aims to improve the properties of metal-ceramic composites and develop new techniques and theories of metal-ceramic composites.
-
The initial model is obtained from the Materials Project [33] database with the entry ID mp-1143. To reduce the lattice mismatch in the following MD simulation, we convert the trigonal Al2O3 to an orthogonal lattice. Consequently, the new Al2O3 cell (60 atoms) has lattice constants of
$ a $ =4.81 Å,$ b $ =8.32 Å,$ c $ = 13.12 Å. The Al2O3 simulation system consists of 22×14×8 unit cells (147840 atoms), with a whole size of 105.71×116.52×104.93 Å3, as shown in FIG. S1 (Supplementary materials, SM).The Matsui potential [34] is adopted for describing the interatomic interaction of the Al2O3 system, which has been widely used in reproducing the structure and mechanical properties of various phases of Al2O3. The potential employs pairwise additive interatomic terms of the form:
in the above equation, the three terms represent Coulomb, van der Waals, and repulsion interactions, respectively. Here
$ {r_{ij}} $ is the interatomic distance between atoms$ i $ and$ j $ , and$ D $ is a parameter with the value of 4.184 kJ·Å−1·mol−1. The effective charge$ q $ , the repulsive radius$ A $ , the softness parameter$ B $ , and the van der Waals coefficient$ C $ , are collected in Table I. And during MD simulation, the long-range Coulombic interactions were calculated by the particle-particle-particle-mesh (PPPM) method [35] with an accuracy of 10−5. -
The unit cell of FeCo (1:1) alloy is built in a cubic lattice using Atomsk [36], with a lattice constant of
$ a $ =$ b $ =$ c $ =2.87 Å (2 atoms). The FeCo alloy simulation system consists of 42×42×42 unit cells (148176 atoms), with a whole size of 120.39×120.39×120.39 Å3, as shown in FIG. S1 (SM). The modified embedded atom method (MEAM) [37] potential is chosen to describe the interactions between Fe and Co. -
For building the Al2O3/FeCo (1:1) interface, two supercells are put together. One supercell with 19×2×5 (91.30×16.65×65.58 Å3) unit cells is constructed from the orthogonal lattice of Al2O3, the other supercell with 32×6×23 (91.72×17.20×65.93 Å3) unit cells is from FeCo alloy. The initial structure contains 20232 atoms for this pair of supercells as shown in FIG. 1. An initial gap between the two surfaces is 2 Å as described in the protocol we used [38]. The degree of the lattice mismatch between the two surfaces is less than 3.32%. And since the height of the Al2O3 side and FeCo side is different, as shown in FIG. 1, a unified length of 65.93 Å is used in the initial structure.
In the simulation of the interface, we use the following hybrid potential. There are three contributions to the potential function: (i) long-range Coulomb potential for all atoms, (ii) Buckingham potential for Al-O and O-O [39] only are collected in Table II, and (iii) Lennard-Jones potential for Al-Al, Al-Fe, Al-Co, Fe-O, Co-O, Fe-Fe, Fe-Co, and Co-Co are collected in Table III [40]. The Ewald summation method is used to calculate the long-range Coulomb interaction with an accuracy of 1.0×10−7.
The Lennard-Jones potential parameters for the cross-interactions between element
$ \alpha $ and element$ \beta $ are estimated using the Lorentz-Berthelot mixing rule [41]:The interaction parameters for Al-Al, Al-Fe, Al-Co, Fe-O, Co-O, Fe-Fe, Fe-Co, and Co-Co are obtained by Eq.(2) and Eq.(3), and the detailed parameters are collected in Table SI (SM).
-
The MD simulation under the magnetic field is implemented using the coupled spin-lattice dynamics methodology [42] in the Large-scale Atomic/Molecular Massively Parallel Simulator (LAMMPS) [43] MD package.
A simple expression for the Hamiltonian of N interacting spins on a fixed lattice is given by [42]:
where
$ {g_i} $ is the Landé factor of the spin$ i $ ,${\mu _0} = 4\pi \times {10^{ - 7}}{\text{ kg}} \cdot {\text{m}} \cdot {{\text{A}}^{{{ - 2}}}} \cdot {{\text{s}}^{{{ - 2}}}}$ is the vacuum permeability, and${\mu _{\text{B}}} = 9.275 \times {10^{ - 24}}{\text{ J}} \cdot {{\text{T}}^{{{ - 1}}}}$ is the Bohr’s magneton. The first term in the formula represents the Zeeman term, which denotes the interaction energy resulting from the spin’s influence on an external uniform magnetic field. The second term corresponds to the exchange interaction term and is expressed as [42]:where the unit of
$ \alpha $ is eV, the unit of$ \delta $ is Å,$ \gamma $ is non-dimensional constant, and${{\Theta }}({{{\boldsymbol R}}_c} - {{{\boldsymbol r}}_{ij}})$ is the Heaviside step function. These three parameters$ \alpha $ ,$ \delta $ , and$ \gamma $ , are to be included in the LAMMPS input files for the simulation under the external magnetic field. In the simulated system, both magnetic metal atoms, Fe and Co, should have these parameters.In this work, the MD simulation without consideration of either atomic magnetism or external magnetic field is denoted as the standard case. We call the situation of Fe and Co with atomic magnetism but without an external magnetic field the magnetism case. The MD simulation with a 5 T external magnetic field is named the magnetic field case.
-
For the pure Al2O3 and pure FeCo alloy systems separately, the initial structure was relaxed at a low temperature of 1 K. When the system reached equilibrium, the temperature was heated up to 300 K and 500 K at a rate of 1.0 K/ps. Then, after reaching equilibrium at 300 K and 500 K for a period of time, the uniaxial tensile simulation was performed in the
$ x $ axis. The tensile rate was 1.0×107 s−1.For the Al2O3/FeCo interface, firstly, the system was equilibrated at 1 K, followed by a heating stage to 300 K and 500 K at a rate of 1.0 K/ps. Then, the 300 K and 500 K structures were equilibrated again in the NPT ensemble separately. Finally, for obtaining Young’s modulus of the interface, uniaxial tensile simulation was carried out for the Al2O3/FeCo interface system. The tensile rate along the
$ x $ axis was 1.0×107 s−1.Periodic boundary conditions were applied in all three dimensions. In this study, we adopted the LAMMPS software to perform MD simulations. The Visual Molecular Dynamics (VMD) [44] package and the Open Visualization Tool (OVITO) [45] package were used for structure monitoring and trajectory analysis.
-
Young’s modulus describes the resistance of solid materials to deformation. For uniaxial tensile, it is a scalar [46]:
where
$ \sigma $ is stress and$ \varepsilon $ is strain. In this work, as described above, we stretch the system along the$ x $ axis, using a constant rate of 1.0×107 s−1, after several trial-and-error tests.The stress-strain curves of pure Al2O3, FeCo alloy, and the Al2O3/FeCo interface at 300 K and 500 K are shown in FIG. 2.
The ridge regression method [47] was used for stress-strain curve fitting to obtain the values of Young’s modulus of pure Al2O3 and FeCo alloy systems. The associated R2, mean square error (MSE), and mean absolute error (MAE) of Al2O3 are 0.9987, 0.0106, 0.0867 at 300 K, and 0.9990, 0.0049, 0.0593 at 500 K. And those of FeCo alloy are R2=0.9998, MSE=0.0013, MAE=0.0321 at 300 K, and R2=0.9986, MSE=0.0084, MAE=0.0778 at 500 K. The MD simulated Young’s modulus in this work, compared with other known results at 300 K, is collected in Table IV. From the current work, the fitted Young’s modulus of Al2O3 is 398 GPa at 300 K, which is in good agreement with the experimental values 370–390 GPa [48], 400 GPa [49], and a reference MD value 396±4 GPa [50]. The fitted Young’s modulus of FeCo alloy is 261 GPa at 300 K, which again corresponds well to an experimental value of 250 GPa [51], a reference MD result of 261 GPa [37], and a first-principle (FP) calculated value of 259 GPa [52]. As the temperature increases, the thermal motion of the atoms intensifies, resulting in a slight decrease in Young’s modulus. The Young’s moduli of Al2O3 and FeCo alloy are 375 GPa and 239 GPa at 500 K respectively. The Young’s modulus of Al2O3 is greater than that of FeCo alloy at both 300 K and 500 K. After all, our result for Al2O3 is within a relative deviation of 0.5%−7.6% compared with the experimental results, and 0.5%−1.5% compared with the other MD result. Our result for FeCo alloy is within a relative deviation of 4.4% compared with the experimental result, and 0.58% compared with the FP calculated result, which is nearly identical to the other MD result.
In the MD simulation results, we also observed that there is a corresponding increase in atomic shear strain with the increase in system strain, as shown in FIG. S2 (SM). The atomic shear strain increases with temperature and is uniformly distributed, which can be attributed to the easier migration of atoms at higher temperatures, resulting in a greater shear strain. No shear bands were monitored during the tensile process, indicating that both Al2O3 and FeCo alloys have good plastic deformation capacities.
The ridge regression method was also exerted in obtaining Young’s modulus of the Al2O3/FeCo interface from our MD simulation. The stress-strain data and fitted curves of the Al2O3/FeCo interface at 300 K and 500 K are shown in FIG. 2. The fitted values are shown in Table IV, with the associated R2=0.9992, MSE=0.0084, MAE=0.0758 at 300 K and R2=0.9991, MSE=0.0088, MAE=0.0753 at 500 K. Compared with Young’s modulus of pure Al2O3 and FeCo alloy systems separately, Young’s modulus of the interface is significantly improved. From FIG. 2, Young’s modulus of the interface is larger than that of both Al2O3 and FeCo alloy at 300 K and 500 K, reaching 577 GPa and 557 GPa respectively. As the temperature increases, the stronger atomic thermal motions lead to a decrease in Young’s modulus of the Al2O3/FeCo interface by approximately 20 GPa.
-
We have then simulated the Al2O3/FeCo interface with the atomic magnetism of Fe and Co, and also activated the external magnetic field for comparison. In this stage, from the MD simulations, the stress-strain curves of the interface were obtained under two different conditions: magnetism case and magnetic field case. The stress-strain results of 300 K and 500 K are shown in FIG. 3 and FIG. S3 (SM). The fitted values of the Al2O3/FeCo interface are shown in Table III. Under condition of magnetism case the associated R2=0.9994, MSE=0.0051, MAE=0.0580 at 300 K and R2=0.9993, MSE=0.0064, MAE=0.0650 at 500 K. Under condition of magnetic field case the associated R2=0.9994, MSE=0.0061, MAE=0.0637 at 300 K and R2=0.9994, MSE=0.0070, MAE=0.0677 at 500 K. Under condition of magnetism case, Young’s modulus of the interface is 615 GPa at 300 K and 606 GPa at 500 K. While under condition of magnetic field case, with a 5 T external magnetic field, Young’s modulus of the interface is 612 GPa at 300 K and 602 GPa at 500 K. Simulation results show that Young’s modulus of the interface is significantly improved by atomic magnetism and external magnetic field.
From FIG. 3 and FIG. S3 (SM), when the strain is set to be 0.005, 0.010, 0.015, the stress is 3.09 GPa, 5.99 GPa, and 8.84 GPa under standard case, 3.37 GPa, 6.47 GPa, and 9.32 GPa under magnetism case, 3.19 GPa, 6.15 GPa, and 9.18 GPa under magnetic field case at temperature of 300 K. And the stress is 2.90 GPa, 5.67 GPa, and 8.38 GPa under standard case, 3.33 GPa, 6.38 GPa, and 9.30 GPa under magnetism case, 3.29 GPa, 6.35 GPa, and 9.26 GPa under magnetic field case at temperature of 500 K. Here we define the stress with a 5 T magnetic field as S5T, that in the magnetism case is Smag, and the stress under standard case as S. And for comparison, we also define two relative stresses: ΔS1=Smag−S and ΔS2=S5T−S. When the strain is 0.005, 0.010, 0.015, the ΔS1 and ΔS2 are shown in Table V.
Simulation results show that the ΔS1 and ΔS2 increase with the increasing strain in the case of magnetism simulation and under a magnetic field. This indicates that the influence of atomic magnetism on the stress-strain curve increases as strain increases. And the higher the temperature, the greater the ΔS1 and ΔS2.
We also compared the shear strain of atoms under different conditions. It can be seen from FIG. 4 and FIG. S4 (SM), that the cases of magnetism and the application of the magnetic field significantly increase the Young’s modulus during the tensile process. For the Al2O3 part, when there is no magnetism or magnetic field, the shear strain of the atoms is smaller compared to the case of atomic magnetism or the magnetic field. In the case of atomic magnetism and the magnetic field, the shear strain of the Al2O3 part increases, but that of the FeCo part slightly decreases. Furthermore, the distribution of shear strain becomes more anisotropic, and shear bands appear in the FeCo part as shown in FIG. 4. The shear strain value of atoms also increases with the rise in temperature. The shear strain of the Al2O3 part is larger than that of the FeCo part. Simulation results show that the atomic magnetism and the magnetic field greatly contribute to the stability of the FeCo part, resulting in a decrease in shear strain and an increase in Young’s modulus at the interface.
-
To explore the details of dynamics at the atomic scale and reveal the mechanism that determines the mechanical responses of the Al2O3/FeCo interface, we calculated the kinetic properties of the interface, including mass density, atom distribution, average density, mean square displacement, diffusion coefficient, and radial distribution function. Considering the structural changes of the interface under different conditions: standard case, magnetism case, and magnetic field case, we calculated the mass density and atom distribution of the Al2O3/FeCo interface using the Fix ave/chunk command in LAMMPS. From FIG. 5 and FIG. S5 (SM), the mass density of the FeCo part is significantly higher than that of Al2O3. At 300 K and 500 K, the number of atoms at the Al2O3/ FeCo interface increases compared to the initial structure. The motion of the atoms in the Al2O3 and FeCo parts causes the interface to combine and fill up the initial gap. With the increase in temperature, atomic motion intensifies and the number of atoms at the interface also increases, indicating a diffusion phenomenon at the interface.
We also investigated the average density of the system under different conditions: standard case, magnetism case, and magnetic field case, as shown in Table VI. The simulated results show a slight increase in the density of the system under conditions of magnetism case and magnetic field case. Under condition of magnetism case, the average density of the Al2O3/FeCo interface increases by approximately 0.5% from 6.40 g/cm3 to 6.43 g/cm3 at 300 K, and increases by approximately 0.9% from 6.38 g/cm3 to 6.44 g/cm3 at 500 K. Under condition of magnetic field case, the average density of the Al2O3/FeCo interface increases by approximately 0.5% from 6.40 g/cm3 to 6.43 g/cm3 at 300 K, and increases by approximately 1.1% from 6.38 g/cm3 to 6.45 g/cm3 at 500 K. It indicates that the atomic magnetism and the external magnetic field result in atom aggregation. The atoms in the interface are more tightly ordered, which also results in an increase in the Young’s modulus of the interface.
To study atomic motion and diffusion of the Al2O3/FeCo interface, the MSD of the atoms is calculated, according to the following equation:
where,
$ {r_i}(t) $ and$ {r_i}(0) $ are the position of the$ i $ -th atom at time$ t $ and 0. To understand the diffusion of the Al2O3/FeCo interface, we calculated the MSD of Al2O3 and FeCo alloy separately. As shown in FIG. S6 (SM), the variation trend of MSD for Al, O, and Al2O3 remains consistent at different temperatures. Still, there are certain differences in the values, the higher the temperature, the larger the MSD values. In the Al2O3 part, the MSD of the O atom is the largest, indicating the O atom moves more vigorously. The MSD of the Al2O3 part is larger than that of the FeCo part. Under a 5 T magnetic field, the MSD of the Al2O3 part increases, while the MSD of the FeCo part decreases. Simulated results show that under the application of the external magnetic field, the Al2O3 part moves more vigorously, and the FeCo part is relatively more stable. Furthermore, the diffusion coefficients, D, of Al2O3 and FeCo alloy were obtained from the MSD results [38],The diffusion coefficients of the Al2O3 part and FeCo part of the interface system are 6.8×10−15 m2/s and 1.4×10−16 m2/s at 300 K, 1.1×10−14 m2/s and 7.2×10−16 m2/s at 500 K. The diffusion coefficient of the FeCo part is smaller than that of the Al2O3 part at the same temperature. Under a 5 T magnetic field, the diffusion coefficients of the Al2O3 part and the FeCo part are 2.3×10−14 m2/s and 2.8×10−16 m2/s at 300 K, 3.8×10−14 m2/s and 1.2×10−15 m2/s at 500 K. Simulated results show that the diffusion coefficients of the Al2O3 part and the FeCo part increase under the external magnetic field. And the FeCo part is more stable than the Al2O3 part. The velocity magnitude of the Al2O3/FeCo interface during the heating stage also indicates that the FeCo part is more stable. From FIG. S7 (SM), the velocity magnitude of the Al2O3 part is significantly greater than that of the FeCo part, combined with the values of MSD and diffusion coefficient, it indicates that the atomic thermal motion of the Al2O3 part is more intense.
To further verify the stability of the interface, the velocity auto-correlation function (VACF) can also be calculated. As shown in FIG. S8 (SM), one property of crystals is that the VACFs typically exhibit oscillatory behavior [53]. The simulated results show that under conditions of magnetism case and magnetic field case, the VACF of Al2O3 and FeCo alloy oscillates more intensely. Moreover, the VACF of Al2O3 oscillates more strongly than that of FeCo alloy.
The RDF,
$ g(r) $ is defined as [54]:where
$ r $ is the distance between a pair of particles,$ p(r) $ is the average number of atom pairs found at a distance between$ r $ and$ r+\mathrm{d}r $ ,$ V $ is the total volume of the system, and$ N\mathrm{_{pairs}} $ is the number of unique pairs of atoms.To study the arrangement of atoms at the interface, we calculated the RDF of the Al2O3 and FeCo parts of the Al2O3/FeCo interface under different conditions at 300 K and 500 K, From FIG. 6 and FIG. S9 (SM), for the Al2O3 part, there is little difference among conditions of standard case, magnetism case, and magnetic field case. With the increase in temperature, the first peak value of RDF decreases from 8.74 Å at 300 K to 8.21 Å at 500 K under condition of standard case, from 8.01 Å at 300 K to 7.75 Å at 500 K under condition of magnetism case, and from 8.04 Å at 300 K to 7.77 Å at 500 K under condition of magnetic field case. For the FeCo part, the atomic magnetism and the external magnetic field have obvious impacts on the value of RDF. The first peak of RDF increases from 23.15 Å under condition of standard case to 35.16 Å under condition of magnetism case and 35.08 Å under condition of magnetic field case. at 300 K, and from 19.84 Å to 31.61 Å and 32.00 Å at 500 K. Furthermore, with an increase in temperature, the atomic thermal motion tends to decrease the peak value of RDF. In the simulation process, lattice distortion occurs in the interface, resulting in a structural transition from body-centered cubic (BCC) phase to hexagonal closest packed (HCP) and a small amount of BCC mixed phase. With increasing temperature, it evolves into a mixture of the HCP phase, face-centered cubic (FCC) phase, and a small amount of BCC phase. The detailed information can be found in the Table SII and FIG. S10 (SM).
-
In summary, in order to study the mechanical properties of the Al2O3/FeCo interface, Young’s modulus of the Al2O3/FeCo interface was calculated by the MD simulation method, and its microstructure characteristics were studied. In addition, the MD simulation under the external magnetic field was successfully realized, and the impact of atomic magnetism and the external magnetic field on the interface microstructure and Young’s modulus was studied. Simulation results show that compared with pure Al2O3 and FeCo alloy, Young’s modulus of the Al2O3/FeCo interface is significantly improved, reaching 577 GPa at 300 K and 557 GPa at 500 K. According to the MSD, RDF, and structure composition of FeCo part, with atomic magnetism and the external magnetic field, the atom aggregation phenomenon of the FeCo part in the Al2O3/FeCo interface is obvious, and its structure is more uniform and stable, which leads to the improvement of Young’s modulus of the Al2O3/FeCo interface. This indicates that the atomic magnetism and magnetic field can effectively regulate the tensile properties of the Al2O3/FeCo interface. This work will help understand the potential use of the Al2O3/FeCo interface in metal-ceramic composite applications, and guide the development of novel metal-ceramic composite materials.
Advances in machine learning have facilitated the development of interatomic interaction potentials. The current machine learning force field includes ACE (atomic cluster expansion) [55], MACE (machine-learned atomic cluster expansion) [56] and deep potential [57], etc. The emergence of the machine learning force field has improved computational efficiency and solved the problem of missing system force fields. We expect the machine learning force field to play a greater role in molecular dynamics simulation in the future.
Supplementary materials: Details of the potential parameters for the Al2O3/FeCo interface; initial simulation models of pure Al2O3 and FeCo alloy; shear strain, MSD, and VACF of Al2O3, FeCo alloy, and Al2O3/FeCo interface; stress-strain curves, mass density, atom distribution, and RDF of Al2O3/FeCo interface at 300 K and 500 K under magnetism case; velocity magnitude of the Al2O3/FeCo interface during the heating stage; structural composition of the FeCo part under different conditions.
Mechanical Properties of Al2O3/FeCo Interface under Magnetic Field: A Molecular Dynamics Study
- Received Date: 22/04/2024
- Available Online: 27/06/2025
-
Key words:
- Molecular dynamics /
- Al2O3/FeCo interface /
- Young’s modulus /
- Magnetism /
- Magnetic field /
- Diffusion coefficient
Abstract: Metal-ceramic composites combine the excellent properties of metals and ceramics, which have high strength, stability, and corrosion resistance. Al2O3/FeCo composites have been proven to be useful in applications such as catalysts, microwave absorption materials, and enhanced permeability dielectric. The understanding of the mechanical properties and dynamics at the atomic scale of the Al2O3/FeCo interface can promote the design and exploitment of metal-ceramic composites. In this work, we have obtained Young’s modulus and diffusion coefficient of the Al2O3/FeCo interface using molecular dynamics simulation, elucidated the structural characteristics of the Al2O3/FeCo interface at the atomic scale, and investigated the impact of atomic magnetism and the external magnetic field on the interface. Simulated results show that Young’s modulus of the Al2O3/FeCo interface is significantly improved compared with pure Al2O3 and FeCo alloy at room and high temperatures. When the atomic magnetism and the external magnetic field are applied, Young’s modulus of the Al2O3/FeCo interface further increases to 612 GPa at 300 K and 602 GPa at 500 K. Moreover, the average density, diffusion coefficient, and radial distribution function are found to be modified substantially. This study will shed light on the atomistic investigations of the metal-ceramic composites.