2025 Volume 38 Issue 6
Article Contents

Shaolin Yang, Cheng Zhen, Panpan Fu, Fangfang Li, Zexi Chen, Jiandong Wu, Hui Lu, Chunping Hou. Novel δ-MnO2/MXene Heterostructures as Cathode Materials for Zinc-Ion Hybrid Supercapacitors[J]. Chinese Journal of Chemical Physics, 2025, 38(6): 947-960. doi: 10.1063/1674-0068/cjcp2408108
Citation: Shaolin Yang, Cheng Zhen, Panpan Fu, Fangfang Li, Zexi Chen, Jiandong Wu, Hui Lu, Chunping Hou. Novel δ-MnO2/MXene Heterostructures as Cathode Materials for Zinc-Ion Hybrid Supercapacitors[J]. Chinese Journal of Chemical Physics, 2025, 38(6): 947-960. doi: 10.1063/1674-0068/cjcp2408108

Novel δ-MnO2/MXene Heterostructures as Cathode Materials for Zinc-Ion Hybrid Supercapacitors

  • Corresponding author: E-mail: slyang@nun.edu.cn; 
  • Received Date: 14/08/2024
    Available Online: 27/12/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(8)

Article Metrics

Article views(144) PDF downloads(0) Cited by(0)

Access History

Novel δ-MnO2/MXene Heterostructures as Cathode Materials for Zinc-Ion Hybrid Supercapacitors

Abstract: Although manganese-based oxide is regarded as a promising cathode material for zinc-ion hybrid supercapacitors (ZHSCs), its practical application is hindered by slow zinc ion diffusion and the instability of MnO2. To overcome this obstacle, a δ-MnO2/MXene heterostructure was created using a simple one-step process under gentle condition. The ZHSC was assembled using this heterostructure as the cathode, activated carbon (AC) as the anode and 2 mol·L−1 ZnSO4 as the electrolyte. The resulting δ-MnO2/MXene//ZnSO4//AC ZHSC shows a maximum specific capacitance of 97.4 F·g−1 and an energy density of 32.27 Wh·kg−1 at the best cathode-to-anode mass ratio. Ex situ characterizations reveal the reversible energy storage mechanism combing Zn2+ insertion/extraction in the cathode, ion adsorption and desorption on the anode surface, and partial reversible formation and dissolution of Zn4SO4(OH)6·5H2O (ZHS) components on both electrodes. Adding of Mn2+ to the electrolyte reduced Mn dissolution, improving the ZHSC’s specific capacitance and energy density to 140.4 F·g−1 and 49.36 Wh·kg−1, respectively, while also enhancing its rate performance and cyclability. The improved electrochemical reaction kinetics was verified through various tests. The results suggest that the δ-MnO2/MXene heterostructure has great potential as a high-performance cathode material for ZHSCs.

    • The pursuit of green and efficient energy storage technologies has occupied the forefront of scientific and technological advancement in recent years [1−3]. Supercapacitors have drawn significant attention because of their high capacity, extraordinary power density, and excellent cyclability [4, 5]. Especially, the hybrid supercapacitor, combining the merits of batteries and capacitors, has been identified as a potential candidate for next-generation energy storage system [6, 7]. Relative to monovalent alkali metal ions, hybrid energy storage devices employing multivalent cations like Al3+, Mg2+, Ca2+, and Zn2+ demonstrate unique advantages, encompassing rapid charge transfer kinetics, elevated specific capacity, and enhanced energy density [8, 9]. In particular, zinc-ion hybrid supercapacitors (ZHSCs) stand out as a new type energy storage device incorporating a zinc-based electrolyte, and both battery-type and capacitor-type electrodes [10−12]. By combining the outstanding characteristics of zinc-ion batteries and supercapacitors, this hybrid device is acknowledged for its high energy density, exceptional cyclic performance, and enhanced safety, positioning it as a highly promising energy storage device [13, 14]. Nevertheless, the distinct energy storage mechanisms of battery-type and capacitor-type electrodes may result in imbalances in specific capacity and electrochemical kinetics between the two electrodes. To organically integrate capacity and rate performance, optimization of current electrode materials and the exploration of novel high-performance alternatives are necessary [15].

      Cathode materials play a critical role in the overall performance of hybrid supercapacitors [15, 16]. Among the various types of cathode materials, MnO2 is notable for its high theoretical specific capacity, ample natural resources, and eco-friendliness [17]. Thus far, the tunnel structure of commercially researched α-MnO2 has been widely explored [18, 19]. In contrast to the tunnel structure, the layered configuration of δ-MnO2 boasts layer-to-layer gaps of up to 0.7 nm and more expansive interlayer channels, rendering it more conducive to Zn2+ storage and release [20]. Furthermore, the diverse oxidation states of Mn (+2, +3, +4), abundant electrochemically active sites and adjustable interlayer spaces confer diverse physicochemical properties upon δ-MnO2 [21]. He et al. reported the preparation of Zn-doped δ-MnO2 (Zn-δ-MnO2) using a hydrothermal method, and the assembled Zn-δ-MnO2//ZnSO4//AC ZHSC exhibits an energy density of 157.2 Wh·kg−1 and power density of 16 kW·kg−1 [20]. Jiang et al. developed a flexible ZHSC assembled by δ-MnO2 cathode, AC anode and PVA-based gel electrolyte, which displays an energy density of 47.86 Wh·kg−1 and power density of 5.81 kW·kg−1 [22]. Nevertheless, low conductivity, structural instability, and volume expansion of MnO2 limit its practical application [23]. Previously, MnO2/carbon nanomaterial composites have been developed to enhance the conductivity and stability of the cathode. For example, Liu et al. reported a ZHSC using graphene nanosheet/carbon nanotube-intercalated nanoflaked manganese dioxide (GNS/CNT@MnO2) as cathode and AC as anode, which deliver an specific capacitance of 105.4 F·g−1 at 0.1 A·g−1 [24]. Bai et al. prepared a porous α-MnO2@reduced graphene oxide (α-MnO2@rGO) cathode, and the ZHSC assembled with α-MnO2@rGO cathode, AC anode and 2 mol·L−1 ZnSO4 electrolyte shows a specific capacitance of 1165.5 mF·cm−2 at a current density of 10 mA·cm−2 [25].

      Recently, MXene, a class of 2D transition metal carbides, carbonitrides, and nitrides, has been demonstrated as an optimal material for compositing with MnO2, due to its high conductivity, abundance, and excellent electrochemical activity [26−30]. Until now, various MnO2/MXene composites have been developed and applied to supercapacitors. For instance, Zhang et al. prepared an MnO2/p-Ti3C2Tx membrane by vacuum filtration of the mixed suspension of porous Ti3C2Tx nanosheets (p-Ti3C2Tx) and hollow MnO2 nanospheres synthesized via a templating-assisted hydrothermal reaction, and the MnO2/p-Ti3C2Tx membrane demonstrated a high specific capacitance of 452 F·g−1 at 1 A·g−1 [31]. Meng et al. presented a method for creating 2D/2D heterojunctions through in situ oxidation involving the growth of α-MnO2 on Ti3C2Tx MXene nanosheets via a 36-h redox reaction at ambient temperature, and the MnO2/MXene heterojunction exhibits an impressive specific capacitance of 334.3 F·g−1 at 0.5 A·g−1 [32]. Liu et al. utilized a hydrothermal approach to synthesize MnO2@MXene composite material, which was then coated onto carbon nanotube fibers (CNTFs). The resulting MnO2@MXene/CNTF demonstrates a remarkable specific capacitance of 181.8 F·g−1 at 1 A·g−1 [33]. However, the actual application of these MnO2/MXene composite materials is hindered by their high-temperature, high-pressure, or complex production processes. Furthermore, to the best of our knowledge, MnO2/MXene composite has not been reported as cathode for ZHSC. Hence, there is a pressing need to devise a straightforward and gentle process for creating high-performance MnO2/MXene composite, which can serve as the cathode material for ZHSC.

      Herein, we reported a δ-MnO2/MXene heterostructure synthesized via a rapid one-step in situ growth method. In the δ-MnO2/MXene cathode, MXene nanosheets, which are highly conductive, serve as an efficient, continuous pathway for electron transport while also effectively preventing the structural collapse of δ-MnO2. Additionally, the combined structure of MXene nanosheets and δ-MnO2 results in a larger specific surface area (SSA) and a more abundant pore structure, providing more electrochemically active sites and shorter ion diffusion paths, thereby enhancing reaction kinetics. A novel ZHSC was constructed, featuring the δ-MnO2/MXene heterostructure as the cathode, activated carbon (AC) as the anode, and a 2 mol·L−1 ZnSO4 serving as the electrolyte. This δ-MnO2/MXene//ZnSO4//AC ZHSC demonstrates a specific capacity of 97.4 F·g−1 and an energy density of 32.27 Wh·kg−1, albeit with a notable lack of cycling stability. Furthermore, the energy storage mechanism of the ZHSC was explored through ex situ X-ray diffraction (XRD), scanning electron microscopy (SEM), and energy dispersive spectroscopy (EDS) tests. The findings reveal a mechanism encompassing the reversible insertion and extraction of Zn2+ ions within the δ-MnO2/MXene cathode, ion adsorption and desorption on the AC anode surface, and the partially reversible generation and dissolution of Zn4SO4(OH)6·5H2O (ZHS) components on both electrodes. Additionally, an attempt was made to mitigate manganese dioxide leaching from the cathode by adding Mn2+ to the electrolyte. The resultant δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC exhibits improvements in maximum specific capacitance and energy density, reaching 140.4 F·g−1 and 49.36 Wh·kg−1 respectively, along with enhanced rate performance and cyclability. These results suggest that the δ-MnO2/MXene heterostructure holds tremendous potential for application in ZHSC, showcasing promising prospects for future use.

    II.   EXPERIMENTS
    • All reagents were commercially available and used without the need for additional purification. Potassium permanganate (KMnO4, ≥98%), sulfuric acid (H2SO4, ≥98%), sodium dodecyl sulfate (SDS, ≥98%), Super-P, polyvinylidene fluoride (PVDF) and N-methyl-2-pyrrolidone (NMP) were purchased from Sinopharm Chemical Reagent Co., Ltd. Beijing. Ti3C2Tx MXene dispersion was obtained from FoShan XinXi Technology Co., Ltd., China. AC was sourced from Fuzhou Yihuan CARBON Co., Ltd., China.

    • Typically, 6.3 mL H2SO4 (0.1 mol·L−1) solution was mixed with 960 mL of sodium dodecyl sulfate (SDS, 0.015 mol·L−1) solution and gently heated to 90 °C for a duration of 15 min. Following this, 2.1 mL Ti3C2Tx MXene dispersion (5 mg·L−1) was introduced into the pre-heated solution. Vigorous stirring for 5 min to guarantee homogenous dispersion, 14.4 mL KMnO4 solution (0.05 mol·L−1) was rapidly added, and the stirring was continued vigorously for another 5 min. Thereafter, the suspension was gently stirred and incubated at 85 °C for 1 h, yielding a brown solution. The δ-MnO2/MXene heterostructure was then extracted through a filtration process of this brown suspension, accompanied by repeated washings with distilled water and ethanol. The final product underwent vacuum drying under 60 °C for 12 h. For comparative analysis, pure δ-MnO2 was crafted using an identical method, albeit without the introduction of MXene.

    • SEM images and EDS mapping were performed on a field emission scanning electron microscope (Zeiss Sigma 500 FESEM). TEM images were observed by a transmission electron microscope (TEM Talos F200X). XRD patterns were recorded with an X-ray diffraction analyzer (Smart Lab SE XRD, operating at 40 kV and 40 mA). Raman spectroscopy was carried out using a Renishaw Invia spectrometer, which employed a laser beam of 633 nm wavelength. Chemical analysis was facilitated by a Thermo ESCALAB 250XI X-ray photoelectron spectrometer for XPS measurements. Fourier transform infrared (FTIR) spectroscopy was carried out on a Nicolet 8700 FTIR spectrometer (Thermo Scientific, Waltham, MA, USA). SSA and pore size were determined through a nitrogen adsorption-desorption test utilizing a Micromeritics APSP 2460 instrument. Mn contents were measured by inductively coupled plasma optical emission spectroscopy (ICP-OES, Optima 7000DV).

    • The cathode slurry was prepared by mixing δ-MnO2/MXene heterostructure or δ-MnO2, super-P, and polyvinylidene fluoride (PVDF) in N-methyl-2-pyrrolidone (NMP) solution at a 7:2:1 mass ratio. Similarly, the anode slurry was created by blending AC, super-P, and PVDF in NMP solution at an 8:1:1 mass ratio. The slurry was evenly coated on the stainless-steel mesh and vacuum-dried at 70 °C for 12 h to obtain cathode and anode, respectively. Once cooled to room temperature, the pieces were pressed by a hydraulic press at 5 MPa for 10 s and then removed for the assembly of the capacitors. Coin cells were assembled using the anode, cathode, a glass fiber (Whatman) membrane separator, and either 2 mol·L−1 ZnSO4 or a mixed 2 mol·L−1 ZnSO4+0.25 mol·L−1 MnSO4 solution utilized as the electrolyte. Galvanostatic charging-discharging (GCD) and galvanostatic intermittent titration technique (GITT) assessments were conducted in a CT 2001A battery testing system (Wuhan Land Electronic Co., Ltd.), operating between 0 and 1.8 V. Cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS) were executed on a CHI 760E electrochemical workstation (Chenhua Instruments, China).

      For CV measurement, the specific capacitance ($ {C}_{m} $ in F·g–1) was computed using the following equation:

      For GCD test, the specific capacitance ($ {C}_{m} $) was calculated using the following equation:

      The energy density (E in Wh·kg–1) and power density (P in W·kg–1) was calculated according to the GCD curve using the formula:

      where i (A·g–1) is the current density of the GCD test, $ \Delta t $ (s) is the discharge time, v is the scan rate, V (V) is the potential, and $ \Delta V $ (V) is the potential window.

    III.   RESULTS AND DISCUSSION
    • The SEM images in FIG. 1(a–c) reveal distinct morphologies for pure δ-MnO2, MXene nanosheets, and δ-MnO2/MXene heterostructure, respectively. Pure δ-MnO2 appears similar to graphene, featuring wrinkled sheets (FIG. 1(a)), whereas MXene nanosheets show a flat structure (FIG. 1(b)). Notably, the δ-MnO2/MXene heterostructure displays a nano-flower structure made up of smaller nanosheets (FIG. 1(c)). EDS elemental mapping verifies the even dispersal of C, Ti, Mn, and O elements within this heterostructure (FIG. 1(d)), suggesting that MnO2 has grown uniformly on the MXene surface. Under TEM examination, pure δ-MnO2 demonstrates a slender sheet-like structure abundant in wrinkles (FIG. 1(e)). In contrast, MXene nanosheets appear as large, transparent flat sheets, typical of a two-dimensional shape (FIG. 1(f)). The TEM image of the δ-MnO2/MXene heterostructure shows a clustered formation of wrinkled and twisted nanosheets (FIG. 1(g)), aligning with SEM observations. Additionally, HRTEM offers a detailed visualization of the δ-MnO2/MXene heterostructure’s microstructure (FIG. 1(h)). Clear lattice fringes are visible in FIG. 1(i), with lattice spacings measuring 0.21 and 0.31 nm that align with the ($ 11\bar{2} $) crystal face of δ-MnO2 (FIG. S1(a) in Sumpplementary materials, SM) and the (006) crystal face of MXene nanosheets (FIG. S1(b) in SM), respectively [28]. This discovery offers proof of the effective creation of the δ-MnO2/MXene heterostructure, showcasing a strong connection between δ-MnO2 and MXene nanosheets.

      As displayed in FIG. 2(a), the XRD spectrum of pure δ-MnO2 samples reveals prominent diffraction peaks at 2θ=12.18°, 24.76°, 36.84°, and 65.96°, which align with the (001), (002), (110), and (020) crystal planes of δ-MnO2 (JCPDS 42-1317), verifying the effective creation of δ-MnO2 [20]. In δ-MnO2/MXene heterostructure, the positions of the (110) and (020) peaks of δ-MnO2 remained unchanged, while the positions of the (001) and (002) peaks of δ-MnO2 slightly shifted to the left and became weaker and wider, indicating that the introduction of MXene increased the interlayer spacing of δ-MnO2 and reduced the layered arrangement of δ-MnO2 layers, promoting the insertion and extraction of zinc ions. Moreover, the (002) peak of MXene vanished at approximately 2θ=6.4°. This phenomenon may result from the in situ binding of MXene nanosheets with δ-MnO2 during the material synthesis, ameliorating the self-stacking behavior of MXene nanosheets induced by interlayer van der Waals forces.

      The Raman spectra of pure δ-MnO2, MXene, and δ-MnO2/MXene heterostructure are depicted in FIG. 2(b). In the spectrum of pure δ-MnO2, peaks at approximately 357 and 645 cm−1 correspond to the skeletal vibration and symmetric stretching of Mn–O bonds within the [MnO6] octahedra, respectively [34]. As for MXene, the strong peak at 199 cm−1 is attributed to the A1g out-of-plane vibration mode. In the spectra of δ-MnO2/MXene heterostructure, the δ-MnO2 peaks are preserved, and the Mn–O bond-associated peak undergoes a blue shift, indicating strengthened Mn–O bonds with MXene introduction [35]. The FTIR spectra of pure δ-MnO2, MXene and δ-MnO2/MXene heterostructure are displayed in FIG. S2 (SM). In the spectrum of pure δ-MnO2, the absorption peak at 555 cm–1 may be attributed to stretching vibration of the Mn–O bond [36]. The peaks at 1531 and 3735 cm–1 should be ascribed to the –OH bending vibrations combined with the Mn atom [37]. MXene shows vibration bands of –OH (3434 cm–1), C=O (1636 cm–1), O–H (1400 cm–1), Ti–O (553 cm–1) [37, 38]. The spectrum of δ-MnO2/MXene heterostructure contains vibration bands of both δ-MnO2 and MXene including –OH (1538, 3428, and 3748 cm–1), C=O (1641 cm–1), Ti–O (522 cm–1), and Mn–O (522 cm–1).

      The XPS full spectrum (FIG. 2(c)) reveals that the major elements in δ-MnO2/MXene heterostructures at different blending ratios are C, Ti, Mn, and O, aligning with the findings from EDS mapping. In the high-resolution XPS spectrum of C 1s for δ-MnO2/MXene heterostructure (FIG. 2(d)), four peaks are observed at 288.6, 286.2, 284.8, and 281.9 eV, corresponding to C=O, C–O, C–C, and Ti–C bonds. The high-resolution XPS spectrum of Ti 2p for δ-MnO2/MXene heterostructure (FIG. 2(e)) reveals three pairs of energy peaks at 459.0 (464.9), 458.3 (463.9), and 457.0 (462.8) eV, signifying the existence of Ti–O, Ti (II), and Ti–C in the heterostructure. The existence of Ti–O bonds can be attributed to the oxygenated groups on the MXene surface [39]. The XPS scan spectrum of Mn 2p (FIG. 2(f)) shows two distinct peaks at 654.0 and 642.4 eV. These peaks correspond to the Mn 2p1/2 and Mn 2p3/2 orbitals, respectively, and exhibit an energy difference of 11.6 eV. This finding further verifies the presence of MnO2 [32, 40]. The XPS scan spectrum of O 1s (FIG. 2(g)) displays four characteristic peaks at 533.2, 531.5, 530.0, and 529.7 eV, representing H–O–H, Mn–OH, Ti–O, and Mn–O–Mn bonds, respectively. The existence of H–O−H bonds can be ascribed to crystalline water in the material [20].

      FIG. 2(h) presents the nitrogen adsorption-desorption isotherms for δ-MnO2 and δ-MnO2/MXene heterostructure. The BET SSA of δ-MnO2/MXene heterostructure is approximately 281.2 m2·g−1, markedly higher than that of pure δ-MnO2 (approximately 23.7 m2·g−1). Moreover, according to the pore size distribution analysis depicted in FIG. 2(i), the δ-MnO2/MXene heterostructure exhibits a broader pore structure than pure δ-MnO2. The increased SSA and abundant pore structure can offer additional active sites for electrochemical reactions, concurrently enhancing electrolyte transport pathways and reducing the diffusion distance of electrolytes, facilitating efficient Zn2+ storage.

    • The performance of the ZHSC is greatly influenced by its voltage window range, which was initially established through electrochemical tests utilizing both the three-electrode and two-electrode systems. FIG. 3(a) illustrates the CV curves of the AC anode and δ-MnO2/MXene cathode, each was tested independently in a 2 mol·L−1 ZnSO4 electrolyte. Evidently, the AC anode displays a rectangular shape, indicative of its typical capacitive behavior within the voltage ranges from −1 V to 0 V. In contrast, the δ-MnO2/MXene cathode remains stable across the voltage window of 0 to 0.8 V, with distinct peaks of oxidation and reduction visible at approximately 0.3 and 0.6 V, respectively, thereby exhibiting pronounced battery-type characteristics. Therefore, it is expected that the assembled ZHSC should operate within the voltage window between 0 and 1.8 V. The GCD profiles of the ZHSCs assembled with various mass ratio of δ-MnO2/MXene cathode to AC anode are displayed in FIG. 3(b). It can be found that the ZHSC reaches maximum specific capacity at mass ratio of 1:1.5. Therefore, the subsequent electrochemical tests were carried out on ZHS assembled with this mass ratio of δ-MnO2/MXene cathode to AC anode. FIG. 3(c) illustrates the CV curves of the δ-MnO2/MXene//ZnSO4//AC ZHSC across various voltage ranges at a sweep rate of 5 mV·s−1. Clearly, the ZHSC experiences water splitting once the voltage surpasses 1.8 V. As a result, the voltage range of 0–1.8 V has been chosen as the optimal window for subsequent electrochemical tests.

      FIG. 3(d) displays the GCD profiles of δ-MnO2//ZnSO4//AC and δ-MnO2/MXene//ZnSO4//AC ZHSCs at 0.2 A·g−1. The specific capacity of the δ-MnO2/MXene//ZnSO4//AC ZHSC is 48.7 mA·h·g−1 (determined by the total mass of active materials in both electrodes), significantly larger than 18.1 mA·h·g−1 of the δ-MnO2//ZnSO4//AC ZHSC. The observed enhancement is credited to the heterostructure that arises from the seamless fusion of δ-MnO2 and MXene nanosheets. This unique structure exhibits superior conductivity, more active sites, and a reduced ion diffusion pathway.

      As seen from the CV curves of δ-MnO2/MXene//ZnSO4//AC ZHSC under various scan rate shown in FIG. 4(a), all curves display a pair of redox peaks with high stability. FIG. 4 (b) and (c) present the GCD curves under varying current densities, the excellent linear voltage-time curves indicate a good capacitive behavior of the ZHSC. The ZHSC achieves a specific capacitance of 97.4 F·g−1 (determined by the total mass of active materials in both electrodes) and an energy density of 32.27 Wh·kg−1 (FIG. S3 in SM) at 0.2 A·g−1.

    • To enhance our comprehension of the energy storage mechanism inherent in the δ-MnO2/MXene//ZnSO4//AC ZHSC and to refine its electrochemical capabilities, a thorough investigation of the electrode reactions occurring on the δ-MnO2/MXene anode and AC cathode was conducted. This exploration was facilitated by ex situ XRD, SEM, and EDS characterizations, aiming to provide deeper insights and pave the way for performance optimization.

      The ex situ XRD pattern evolution of the δ-MnO2/MXene cathode is presented in FIG. 5(a). In comparison to its original state, distinct peaks for Zn4SO4(OH)6·5H2O (ZHS, JCPDS 78-0246) and ZnMn3O7·3H2O (JCPDS 15-0807) emerge after full discharge. The appearance of ZHS might be due to H+ ions infiltrating the δ-MnO2/MXene cathode during discharge, elevating its surface pH value. Additionally, the presence of ZnMn3O7·3H2O indicates a structural shift from layered δ-MnO2 to spinel-type ZnMn2O4, involving Mn in both intermediate (III) and (II) states, during the intercalation of Zn2+ into the δ-MnO2/MXene cathode [20]. Furthermore, the absence of the prominent ZHS peak when fully charged, presumably due to its dissolution during the charging process, underscores the reversibility of the ZHS compound within the cathode throughout the charging and discharging cycles.

      The morphological changes of the δ-MnO2/MXene cathode during the charge/discharge cycle were carefully observed using SEM (FIG. 5(b)). Evidently, distinct ZHS flakes emerge on the surface of the δ-MnO2/MXene cathodes upon full discharge. EDS mapping further confirms the homogenous dispersal of Mn, O, Zn, and S elements (FIG. S4 in SM), thereby affirming the creation of ZHS. Notably, these flakes vanish after the cathode is fully charged, suggesting that ZHS dissolves in the charging phase. This observation underscores the reversible character of ZHS formation and dissolution.

      The variation of the AC anode was also characterized by ex situ XRD (FIG. 5(c)). Initially, the AC cathode solely displays the distinctive diffraction peaks of carbon, which are broad and indicate low crystallinity. Upon full charge, the XRD pattern of the AC anode reveals a prominent characteristic peak associated with Zn4SO4(OH)6·5H2O (ZHS, JCPDS 78-0246). Nevertheless, the diminished ZHS signal in the fully discharged state hints that ZHS may not entirely dissolve in the electrolyte. Additionally, deposits of ZnSO4·xH2O (as identified by JCPDS 22-1018) were detected on the anode surface [41]. These findings implicate that the zinc ion concentration in the electrolyte could potentially decline during prolonged cycling, subsequently impacting the cycling stability of the ZHSC.

      As the SEM images displayed in FIG. 5(d), the original AC anode consists of micrometer-sized AC particles. Upon full charging, numerous ZHS flakes emerge on the surface of AC anode. The homogenous dispersal of Mn, O, Zn, and S elements, as evidenced by EDS mapping, corroborates the formation of ZHS (FIG. S5 in SM). Furthermore, minimal quantities of Mn elements were identified on the surface, suggesting that Mn from the cathode dissolves in the electrolyte during charging and partially deposits electrochemically on the anode surface. This observation points to another potential reason for the subpar recyclability of ZHSC. Upon examination of the SEM image of the fully discharged AC electrode, flaky substances are still visible on its surface, highlighting the poor reversibility of ZHS generation and dissolution on the anode throughout the charging/discharging process. This, in turn, contributes to the loss of the zinc source in the electrolyte.

      Given the AC anode’s high SSA and suitable pore size, adsorption and desorption of ions on the surface of AC particles is unavoidable. Therefore, the charge storage mechanism of ZHSC is identified to involve reversible intercalation and deintercalation of Zn2+ into and from the δ-MnO2/MXene cathode, ion adsorption and desorption on the surface of the AC anode, as well as partially reversible participation and dissolution of ZHS components on both electrodes.

    • To hinder the dissolving of manganese, Mn2+ was introduced into the electrolyte by employing a 2 mol·L−1 ZnSO4 and 0.25 mol·L−1 MnSO4 solution. Subsequently, a comprehensive exploration of the electrochemical behavior of the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC system was undertaken. FIG. 6(a) portrays the CV curves of the ZHSC at diverse scan rates, showcasing consistent operation within the 0–1.8 V voltage range and maintaining distinguishable redox peaks. In contrast to the δ-MnO2/MXene//ZnSO4//AC ZHSC devoid of Mn2+, the redox peaks appear broader, suggesting an enhancement in capacitive behavior. As scan rates increase, the CV curve retains its form without significant distortion, demonstrating excellent rate performance.

      The rate performances of ZHSCs assembled with both electrolytes are presented in FIG. 6(b). The δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC achieves a high specific capacitance of 142.9 F·g−1 at a scanning rate of 2 mV·s–1, exceeding the 90.1 F·g−1 of the δ-MnO2/MXene//ZnSO4//AC ZHSC, thus demonstrating a notable capacity increase. At an elevated scan rate to 100 mV·s–1, the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC maintains a specific capacitance of 51.2 F·g−1 and a capacitance retention rate of 35.8%, considerably higher than 25.6% (23.1 F·g−1) of the δ-MnO2/MXene//ZnSO4//AC ZHSC.

      FIG. 6 (c) and (d) exhibit the GCD profiles of the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC across various current densities. These profiles reveal a more symmetrical shape in comparison to the δ-MnO2/MXene//ZnSO4//AC ZHSC, indicating excellent reversibility in the charge/discharge process. Furthermore, the extended discharge duration at equivalent current densities implies a higher specific capacitance when juxtaposed with the δ-MnO2/MXene//ZnSO4//AC ZHSC. Specifically, the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC displays a remarkable specific capacitance of 140.4 F·g−1 and an improved energy density of 49.36 Wh·kg−1 (FIG. S3 in SM) when tested at 0.2 A·g−1. The augmented capacitive performance is due to the deposition and dissolution of Mn2+ present in the electrolyte during charge-discharge cycles, thereby contributing to the overall capacity [42, 43]. This specific capacitance surpasses many manganese based ZHSCs, such as, MnO2//Zn(CF3SO3)2//AC ZHSC (83.52 F·g−1 at 0.1 A·g−1) [44], GNS/CNT@MnO2//ZnSO4+MnSO4//AC ZHSC (105.4 F·g−1 at 0.1 A·g−1) [24], MnO2-CNT//ZnSO4+MnSO4//MXene ZHSC (115.1 F·g−1 at 1 mV·s−1) [18], δ-MnO2//PVA-ZnSO4//AC FZHSC (53.18 F·g−1 at 1 mA·cm−2) [22], MnO2@CC//ZnCl2@MnSO4/PVA//AC@CC ZHSC (70.57 F·g−1 at 1 mA·cm−2) [45]. The cyclability of both ZHSCs were assessed by repeating the CV scans at 50 mV·s–1, and the result is shown in FIG. S6 (SM). After undergoing 2000 cycles, δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC maintains a capacitance retention of 79.56%, much higher than 57.73% of δ-MnO2/MXene//ZnSO4//AC ZHSC. ICP-OES measurements were conducted to compare the variation of Mn contents in the cathodes of both ZHSCs after cycling. The Mn content in the original δ-MnO2/MXene is 32.92%. After 2000 cycles, the Mn content in the cathode of δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC slightly decreases to 30.74%, while that of δ-MnO2/MXene//ZnSO4//AC ZHSC reduces to 21.2%. This result suggests that the addition of Mn2+ in the electrolyte mitigates the dissolution of Mn in a larger extent.

      To understand the reasons behind the better rate performance of the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC, we conducted a thorough examination of the electrode reaction kinetics. The peak current (i) and scan rate (v) relationship adheres to the formula $i=av^{b}$, where b usually falls between 0.5 and 1.0. Specifically, a b value of 0.5 represents a diffusion-controlled process, whereas a b value of 1.0 denotes a capacitance-controlled process. As illustrated in FIG. 7(a), the δ-MnO2/MXene//ZnSO4//AC ZHSC has b values of 0.80 and 0.71 for peaks of oxidation (O) and reduction (R), respectively, as calculated from the slope of the fit lines relating logi and logv. In contrast, the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC exhibits b values of 0.93 and 0.81 for peaks of oxidation and reduction, respectively (FIG. 7(d)). These higher b values, which are closer to 1, indicate an enhanced capacitive behavior in the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC, suggesting a more pronounced capacitive response in this configuration.

      To obtain a more quantitative evaluation of capacitance contribution, calculations were performed using the formula $i\left(v\right)={k}_{1}v +{k}_{2}v^{1/2}$, wherein ${k}_{1}v$ signifies the capacitance-controlled component, while ${k}_{2}v^{1/2}$ denotes the diffusion-controlled component. This methodology facilitates the derivation of capacitance contribution ratios across various scanning rates. As the scanning rate escalates from 2 mV·s–1 to 100 mV·s−1, the capacitance contributions for δ-MnO2/MXene//ZnSO4//AC ZHSC augment from 23.3% to 90.9% (FIG. 7(b)). Similarly, for the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC, the contributions climb from 34.1% to 95.2% (FIG. 7(e)). Broadly speaking, the capacitance contribution ratios of the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC prove superior to those of the δ-MnO2/MXene//ZnSO4//AC at each scan rate, thereby highlighting an improved capacitive performance. Specifically, as illustrated in FIG. 7(c), at a scanning rate of 5 mV·s−1, the capacitance contribution for the δ-MnO2/MXene//ZnSO4//AC stands at 29.4%, whereas it jumps to 39.8% in the case of the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC (FIG. 7(f)). These observations strongly suggest that the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC displays enhanced electrochemical kinetics, bestowing it with superior rate performance.

      To acquire a profound understanding of how the introduction of Mn2+ into the electrolyte affects the kinetics of electrochemical reactions, EIS and GITT tests were conducted. As seen from the Nyquist plots presented in FIG. 8(a), the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC exhibits a smaller semicircle diameter in the high-frequency regime, which indicates reduced charge transfer resistance and augmented charge transfer efficiency. Furthermore, FIG. 8(b) demonstrates a linear relationship of Z′ versus ω−1/2 in the low-frequency range for both types of ZHSCs. Through linear fitting, we obtained slopes of 41.13 and 30.01 for the δ-MnO2/MXene//ZnSO4//AC and δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSCs, respectively. The flatter slope observed in the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC signifies smaller Warburg coefficients (σ), pointing to an improved ion diffusion capacity.

      The GITT profiles, along with the associated diffusion coefficients, for both ZHSCs are presented in FIG. 8(c). For the δ-MnO2/MXene//ZnSO4//AC ZHSC, the diffusion coefficient varies from 10−9 cm2·s−1 to 10−11 cm2·s−1 during discharge and from 10−9 cm2·s−1 to 10−13 cm2·s−1 during charge. By contrast, the δ-MnO2/MXene//ZnSO4 + MnSO4//AC ZHSC (FIG. 8(d)) demonstrates a diffusion coefficient between 10−9 cm2·s−1 and 10−10 cm2 s−1 during discharge, and between 10−9 cm2·s−1 and 10−12 cm2·s−1 during charge. Evidently, the δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC boasts superior diffusion coefficients during both charging and discharging, indicating a notably higher ion diffusion rate compared to the δ-MnO2/MXene//ZnSO4//AC ZHSC.

    IV.   CONCLUSION
    • In conclusion, we proposed a mild and facile method to prepare δ-MnO2/MXene heterostructure through a one-step reaction. The ZHSC assembled with δ-MnO2/MXene cathode, AC anode and 2 mol·L−1 ZnSO4 electrolyte shows a specific capacitance and energy density of 97.4 F·g−1 and 32.27 Wh·kg−1 at 0.2 A·g−1, respectively. Ex situ XRD, SEM, and EDS characterizations revealed the charge storage mechanism of ZHSC encompassing the reversible intercalation and deintercalation of Zn2+ ions into and out of the δ-MnO2/MXene cathode, ion adsorption and desorption processes on the surface of the AC anode, along with the partially reversible generation and dissolution of ZHS components on both electrodes. The electrochemical performance of the ZHSC was optimized by adding Mn2+ ions into the ZnSO4 electrolyte. The δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSC displays a notable specific capacitance of 140.4 F·g−1, an enhanced energy density of 49.36 Wh·kg−1 at 0.2 A·g−1, along with significantly improved rate performance and cyclability. Subsequently, electrochemical kinetics studies were conducted on the two electrolyte systems, confirming that the addition of Mn2+ effectively improved the electrochemical reaction kinetics, laying a scientific foundation for further optimizing this ZHSC system. These results demonstrate the potential application of δ-MnO2/MXene heterostructure in the field of ZHSCs.

      Sumpplementary materials: HRTEM images of pure δ-MnO2 and MXene, FTIR spectra of pure δ-MnO2, MXene and δ-MnO2/MXene heterostructure, Ragone plots and cyclic stability of the δ-MnO2/MXene//ZnSO4//AC and δ-MnO2/MXene//ZnSO4+MnSO4//AC ZHSCs, and EDS mapping of the δ-MnO2/MXene and AC cathodes in the fully discharged state.

    Figure (8)  Reference (45)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return