The electrochemical reduction of carbon dioxide (CO2RR) presents a promising and sustainable pathway for converting greenhouse gases into valuable fuels, offering the dual benefits of carbon mitigation and energy storage [1, 2]. Recent advancements in electrocatalysis have significantly improved the efficiency and selectivity of CO2RR catalysts, primarily through the optimization of local microenvironment including catalyst geometries and the fine-tuning of active site configurations [3−6]. However, to fully unlock the industrial potential of CO2RR, further rational design is necessary to continue enhancing both catalytic activity and selectivity [7−15]. In this regard, atomically dispersed metal catalysts, particularly single-atom catalysts, have garnered considerable attention due to their uniform atomic structures, well-defined active sites, and improved metal utilization efficiency [16−21]. Despite these advantages, the inherent complexity of CO2RR, involving multi-electron and multi-proton transfer processes, frequently necessitates cooperative interactions among metal sites. This presents a significant challenge for conventional carbon-nitrogen-supported single-atom catalysts, as their isolated metal sites limit their ability to efficiently activate CO2 and enhance catalytic selectivity.
Alternatively, SAAs have emerged as promising catalysts in energy applications due to the unique synergistic effects arising from the interaction between host nanoparticles and dispersed guest metal atoms. These interactions offer significant advantages for multi-site catalysis, enhancing both activity and selectivity in CO2 reduction [22−27]. Nevertheless, the high surface energy of SAAs often leads to significant alterations in the local microenvironment under working conditions, driven by applied voltage and interactions with reaction intermediates [28−34]. This structural susceptibility complicates the detailed investigation of rearrangements at active sites, posing a substantial challenge to understanding their working mechanism. Consequently, real-time monitoring of the dynamic changes in SAAs and their interactions with intermediates is highly desirable, yet remains a considerable challenge. Fortunately, advancements in high-brightness synchrotron radiation techniques offer new opportunities for dynamic monitoring of the local environment. Among them, structure-sensitive XAS provides key insights into the coordination and electronic states of active sites, while SR-FTIR enables precise detection of surface-adsorbed intermediates [35−39]. These techniques allow for real-time, atomic-scale insights into the dynamic evolution of active sites, facilitating a more comprehensive understanding of the structure-activity relationship in SAAs.
This study presents a SAA catalyst, Co1Ox@Au, for CO2RR, synthesized via a co-precipitation method, achieving a notable CO selectivity of 92.2%. By combining operando XAS and SR-FTIR, we gain a deeper insight into the voltage-driven behavior of Co1Ox@Au. Our findings reveal that the single-atom Co, firmly anchored on the surface of Au nanoparticles, undergoes significant dynamic changes to form the Co1@Au active site when subjected to applied voltages. Compared to unmodified Au nanoparticle, this voltage-induced evolution in Co1Au leads to a strengthening of the Co-Au interaction, which in turn modulates the electronic properties of the active sites. This strengthened bimetallic interaction plays a crucial role in facilitating the adsorption of the *COOH intermediate, a crucial step in the CO2RR process. Furthermore, it accelerates the desorption of *CO, ensuring efficient CO formation. Both effects are essential for achieving the observed enhanced CO selectivity. This work highlights the critical role of atomic-scale interactions in optimizing catalyst performance and offers new perspectives for the design of CO2RR catalysts.
-
Co1Ox@Au was synthesized through the co-precipitation of metal precursors. In a typical synthesis, 0.075 mmol of cobalt acetylacetonate (Sigma Aldrich) and 0.9 mmol of chloroauric acid tetrahydrate (Sinopharm Group) were added into 8 mmol of oleylamine (Sigma Aldrich). The mixture was then ultrasonicated to form the uniform precursor solution. Next, the solution was mixed with 20 mL of glycol (Sinopharm Group) under vigorous stirring in a round flask, followed by bubbling of nitrogen for 30 min to remove dissolved oxygen. Under the nitrogen atmosphere, the solution was heated to 180 °C for 2 h with reflux and then cooled naturally. Afterward, 50 mL of ethanol (Sinopharm Group) was added to the solution to precipitate the synthesized NPs. The NPs were then washed with hexane (Sinopharm Group) three times by centrifugation and dried under vacuum.
The prepared Co1Ox@Au NPs were loaded on XC-72 carbon powder support material at a ratio of 20 wt% (based on the total mass of Co and Au) for further characterizations. The XC-72 carbon powder was ultrasonicated in n-butylamine (Sigma Aldrich) for 30 min. Then, the isolated NPs were redispersed in the XC-72/n-butylamine suspension. This final mixture was then magnetically stirred for one day. Finally, the mixture was magnetically stirred for another 24 h and washed with ethanol three times by centrifugation and dried under vacuum.
-
X-ray diffraction (XRD) patterns were obtained using a Philips X’pert Pro Super diffractometer. Transmission electron microscopy (TEM) was carried out on FEI-30 ESEM and JEOL-2100F to characterize the morphologies of samples. Energy-dispersive X-ray spectroscopy (EDS) for elemental mapping was carried out with a 26FEI Talos F200X. High-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) and high-resolution TEM were conducted with a JEM-ARM 200F instrument. The concentrations of Co and Au atoms were measured directly by inductively coupled plasma optical emission spectroscopy (ICP-OES) (Optima 7300 DV).
-
Electrochemical measurements were performed using a three-electrode system. The gas-tight flow cell was designed with a CO2 gas compartment and two liquid compartments. The catholyte and anolyte were separated by an anion exchange membrane. The catalyst ink was prepared by dispersing the catalyst powder in a solution of deionized water, isopropanol, and Nafion (5 wt%) as a binder. The suspension was ultrasonicated for 30 min to ensure uniform distribution. The ink was then drop-cast onto a gas diffusion electrode (GDE, TGPH060H Hydrophilic Carbon Paper) and dried at ambient temperature. Before CO2RR testing, the catalyst underwent an electrochemical reduction pre-treatment. This involved holding the electrode at −0.6 V vs. RHE for 10 min in a CO2-saturated 0.5 mol/L KHCO3 solution to activate the catalyst surface and reduce any oxide layers present. Effluent gases were collected and analyzed using gas chromatography. Liquid products were quantified using 1H NMR spectroscopy in a water suspension. Further details on the CO2 reduction reaction (CO2RR) performance test are available in Supplementary materials (SM).
-
Co K-edge (7112 eV) and Au L3-edge (11919 eV) X-ray absorption spectroscopy (XAS) measurements were conducted at the 1W1B beamline of the Beijing Synchrotron Radiation Facility (BSRF), China. To minimize harmonics, the X-ray beam was detuned by 30% for the Co K-edge and 15% for the Au L3-edge. Operando XAS was carried out in a custom-built cell, with the catalyst-coated carbon fiber paper used as the working electrode, secured with polyimide film to ensure full interaction with the KHCO3 electrolyte. Additional details on the XAS analysis can be found in SM.
-
Co1Ox@Au nanoparticle was synthesized via a co-precipitation method. FIG. 1(a) presents TEM images, which clearly reveal a well-dispersed array of spherical nanoparticles. These nanoparticles exhibit diameters that fall within a range of 7.0 nm to 9.0 nm, indicating a consistent size distribution. To delve deeper into their structural properties, high-resolution TEM (HR-TEM) analysis was conducted. This analysis confirmed lattice spacings of 0.24 nm and 0.20 nm, which correspond to the Au(111) and Au(200) planes, respectively, as illustrated in FIG. S1(a, b) of SM. This observation is consistent with the XRD result (FIG. S2 in SM). Furthermore, HAADF-STEM images, presented in FIG. 1(b), uncover the presence of notable defects within the Au nanoparticles. These defects include twin boundaries and dislocations, highlighting the complex internal structure of the nanoparticles. It is worth noting that the Co sites within the Au nanoparticles are observed as regions of low brightness, with no indication of significant Co aggregation (FIG. 1(c)). To further validate the uniform distribution of Co atoms within the Co1Ox@Au nanoparticles, elemental mapping was performed using EDS. As depicted in FIG. 1(d), the EDS results confirm a homogeneous dispersion of Co atoms throughout the nanoparticles. The atomic ratio of Au to Co was meticulously measured and found to be 97:3, which agrees with the data obtained from ICP-OES of 96.4:3.6. Considering the low Co content and its homogeneous distribution, it is reasonable to suggest that Co is predominantly dispersed in an isolated state within the Au nanoparticles.
Subsequent characterization of the local structure of Co1Ox@Au SAA was conducted using XAS measurements. The X-ray absorption near edge structure (XANES) spectra, which were recorded at the Co K-edge, are presented in FIG. S3 (SM). These spectra reveal a notable shift in the absorption edge (E0) of Co1Ox@Au towards higher energy when compared to that of Co foil. Additionally, the XANES spectra exhibit a pre-edge peak at 7712 eV, which is more pronounced than that observed in Co2O3. This heightened peak indicates an increased probability of 1s-3d transitions occurring within the Co1Ox@Au SAA. Furthermore, the broadening of the absorption peak observed in the XANES spectra points to a change in the local symmetry surrounding the Co atoms, indicating a unique local microenvironment for the Co species in the Co1Ox@Au SAA. To further elucidate the atomic structure of the Co1Ox@Au SAA, Fourier-transform extended X-ray absorption fine structure (FT-EXAFS) spectra were recorded at both the Co K-edge and Au L3-edge. As displayed in FIG. 1(e), the FT-EXAFS spectra of Co1Ox@Au SAA exhibit a prominent peak at 1.56 Å, which corresponds to Co-O coordination. Another coordination peak, observed at 2.19 Å, could be attributed to either Co-Co or Co-Au coordination, however, making a precise distinction challenging. Given the HAADF-STEM results, which demonstrate that Co is present as isolated atoms embedded within the lattice of Au nanoparticles, it is reasonable to attribute this peak at 2.19 Å to Co-Au interaction. Additionally, a metallic coordination peak appears at 2.86 Å, which is also attributed to Co-Au coordination. The splitting of these two peaks, both from the Co-Au coordination shell, arises due to the strong scattering effect of the Au atoms [40−42]. Furthermore, a peak at 1.98 Å, corresponding to Au-Co/Au coordination, is observed in FIG. 1(f). This combined microscopy and XAS analysis provides strong evidence for the Co atoms in the Co1Ox@Au SAA existing as isolated Co1Ox species anchored onto the surface of the Au nanoparticles.
The evaluation of the CO2RR performance of Co1Ox@Au SAA using a gas diffusion electrode (GDE) as the substrate for both Co1Ox@Au and Au nanoparticles (Au NPs) reveals notable enhancements in catalytic activity. Specifically, linear sweep voltammetry (LSV) measurements, as depicted in FIG. 2(a), reveal a striking disparity in total current density between Co1Ox@Au SAA and Au NPs. At an applied potential of −0.6 V versus the reversible hydrogen electrode (RHE), Co1Ox@Au SAA attains a substantially higher current density of 12.5 mA/cm2, indicating its enhanced electrocatalytic prowess in converting CO2. This enhanced performance is further corroborated by the Faradaic efficiency (FE) for CO production, shown in FIG. 2(b). Across the potential range spanning −0.6 V to −0.8 V vs. RHE, Co1Ox@Au SAA consistently maintains an FE for CO above 80%, peaking at approximately 92.2% at −0.75 V vs. RHE (Table S1 in SM). This high efficiency underscores its ability to selectively convert CO2 into CO. As the applied potential is increased, the Faradaic current for CO rises accordingly, reaching a plateau at −0.8 V vs. RHE. The minor decline in CO selectivity at this potential is attributed to the onset of the competing hydrogen evolution reaction, which contributes to an elevated overall current density without a corresponding increase in the current specifically attributed to the CO2RR. Thus, the optimal reduction potential for CO2RR on Co1Ox@Au SAA is deemed to be −0.8 V vs. RHE, balancing high CO production with minimal interference from HER. In stark contrast, Au NPs of comparable size, but devoid of the single-atom Co modification, demonstrate a significantly reduced CO selectivity of around 41.5%. This disparity underscores the pivotal role of the Co1Ox modification in enhancing the catalytic activity of the Au nanoparticles.
An intermediate-sensitive operando SR-FTIR analysis was performed to investigate the adsorption and desorption behavior of crucial intermediates formed during the CO2RR on the Co1Ox@Au SAA. The experimental configuration, as illustrated in FIG. 2(c), comprised a three-electrode electrochemical cell equipped with a glassy carbon working electrode (WE), an Ag/AgCl reference electrode (RE), and a Pt wire counter electrode (CE), all immersed in a 0.5 mol/L KHCO3 electrolyte solution. Upon applying cathodic potentials of −0.2 V and −0.8 V vs. RHE, distinct infrared absorption bands emerge in the spectral region, specifically at wavenumbers of approximately 2356 cm−1, 1758 cm−1, and 1980 cm−1 (FIG. 2(d–f)). Notably, the absorption bands observed at 1758 cm−1 and 1778 cm−1 are attributed to the stretching vibrations of the *COOH intermediate, a key species in the CO2RR pathway. Meanwhile, the peak at 2356 cm−1 is assigned to the symmetric stretching of adsorbed *CO2, indicating the presence of CO2 molecules on the catalyst surface [43−46]. Under open-circuit voltage (OCV) conditions, a pronounced peak of *CO2 is evident. As the applied potential shifted from −0.2 V to −0.8 V vs. RHE, a notable decrease in *CO2 adsorption is observed, accompanied by an increase in the adsorption of the *COOH intermediate. This change indicates an intensified reaction progression and a more favorable environment for the stabilization of the *COOH species. At −0.8 V vs. RHE (FIG. 2(e)), the *COOH band exhibits a high-wavenumber shift. This blueshift suggests a stronger adsorption of the *COOH intermediate on the Co1Ox@Au SAA [47].
Moreover, the SR-FTIR spectra recorded at −0.2 V vs. RHE reveal an additional band centered around 2013 cm−1, which corresponds to the adsorption of *CO (FIG. 2(f)). This band undergoes a progressive redshift to 1980 cm−1 as the cathodic potential is increased from −0.2 V to −0.8 V vs. RHE in the presence of CO2. The redshift, accompanied by a decrease in band intensity, suggests a reduction in the surface coverage of *CO. This observation indicates facilitated desorption of *CO and the efficient release of CO as the final product of the CO2RR process, which is frequently considered challenging [48−50]. Accordingly, these results offer valuable insights into the CO formation pathway during CO2RR on the Co1Ox@Au SAA. Initially, CO2 molecules adsorb onto the active sites and are activated to form the *COOH intermediate, which is further protonated, ultimately leading to the desorption of CO. The optimized adsorption of *COOH and the easier desorption of *CO observed on the Co1Ox@Au SAA, suggest an enhanced catalytic performance (FIG. 2(g)). This proposed enhancement mechanism is consistent with the reduction current observed in the LSV curves.
To clarify the variations in the local microenvironment of Co1Ox@Au, operando XAS measurements were conducted under CO2RR conditions. FIG. 3(a) presents the XANES spectra of Co1Ox@Au alongside Au foil as a reference. The similarity of the spectral features at potentials of −0.2 V and −0.8 V vs. RHE, and post-reaction state indicates the structural robustness of Co1Ox@Au during CO2RR. In the inset of FIG. 3(a), the white-line peak at 11923 eV in the Au L3-edge XANES spectra, associated with the electron transition from the Au 2p orbital to the partially filled 5d orbital, exhibits a higher intensity than that of Au foil. This observation suggests that the incorporation of single-atom Co into the Au nanoparticles induces a partial vacancy in the Au 5d orbital, implying electron transfer between Au and Co atoms. Furthermore, the FT-EXAFS spectra in FIG. 3(b) reveal that the Au-Au coordination peaks are similar to those of Au foil, reinforcing the notion that Co1Ox@Au SAA retains a stable structure, with Co atoms existing as single atoms at low concentrations during the CO2RR. Therefore, the enhanced CO2RR activity of Co1Ox@Au can be attributed to electronic interactions between Au and Co atoms.
FIG. 3(c) depicts the Co K-edge XANES spectra of Co1Ox@Au SAA under various reaction conditions, with a Co foil as reference. At first glance, a gradual increase in the intensity of the pre-edge peak with more negative applied potentials suggests a simultaneous decrease in the structural symmetry of Co site. At −0.8 V vs. RHE, the pre-edge peak at 7712 eV, corresponding to the 1s to d-p hybridized orbital transition, acts as a fingerprint for local symmetry. Additionally, the E0 position shows a low-energy shift by 2.2 eV, suggesting a reduction in the Co oxidation state during CO2RR. After the reaction, the E0 does not fully return to its original position, implying irreversible changes in the single-atom Co site. Further insights from the FT-EXAFS spectra (FIG. 3(d)) reveal that the initial Co-O coordination at 1.56 Å diminishes during the CO2RR, while Co-Au coordination peaks at 2.19 Å and 2.86 Å, become more notable. These observations suggest that Co undergoes gradual reduction during CO2RR process, reducing the surrounding O atoms and exposing Co atoms, which subsequently form direct coordination with Au atoms within the nanoparticle. This self-optimizing behavior strengthens the Co-Au interaction, optimizing the geometric and electronic configurations of SAA, ultimately enhancing CO2RR activity and selectivity.
To accurately determine the oxidation state of Co during the CO2RR process, a valence-state linear fitting analysis was performed on the operando XANES spectra. This analysis was referenced to the E0 positions of Co foil (Co0) and Co2O3 (Co3+) standards, as shown in FIG. 4(a). Using the E0 values of Co0 (7709 eV) and Co3+ (7722.74 eV, with a ΔE0 shift of 13.74 eV), a regression line was generated to correlate various oxidation states [52]. At −0.2 V vs. RHE, the oxidation state of Co was determined to be +2.74. As the potential was further reduced to −0.8 V vs. RHE, the oxidation state dropped to +2.53, and it further decreased to +2.27 after the reaction. These results indicate that under reduction voltages, Co assumes a distinctive local geometry and a lower oxidation state, contributing to the improved CO2RR performance.
For deeper insights into the structural evolution of Co1Ox@Au SAA, EXAFS fitting was performed (FIG. 4(b), FIG. S4 (SM) and Table S2 (SM)) [53]. At an initial potential of −0.2 V vs. RHE, the Co site is predominantly coordinated with oxygen (Co-O), showing a coordination number of 3.1 and a bond length of 1.98 Å. Upon applying a more negative reduction potential of −0.8 V vs. RHE, the Co-O coordination number decreases sharply to 0.8 and further drops to 0.5 after completing the CO2RR, suggesting substantial structural changes at the Co sites. However, at −0.8 V vs. RHE, fitting with only Co-O and Co-Au paths was insufficient to fully capture the structural evolution, requiring the inclusion of additional Co-Au coordination pathways. This involves Co-Au1 coordination at the surface and Co-Au2 coordination within the nanoparticle. The inclusion of these three paths significantly improved the fitting results for the −0.8 V vs. RHE and after-reaction state. Specifically, at −0.8 V vs. RHE, the coordination number for Co-Au1 is determined to be 5.8, with a bond length of 2.61 Å, while Co-Au2 exhibits a coordination number of 7.1 and a bond length of 2.82 Å. After the reaction, the coordination number for Co-Au1 slightly decreases to 5.5, with a bond length of 2.66 Å, and Co-Au2 has a coordination number of 7.0 with a bond length of 2.85 Å, indicating that the Co-Au coordination structure remains stable throughout the process. This refined analysis reveals the progressive structural changes that occur during CO2RR, with more single-atom Co interacting with Au within the nanoparticles, thus optimizing the adsorption and desorption towards the *COOH and *CO, as confirmed by operando SR-FTIR.
As illustrated in FIG. 4(c), the fitting results suggest that the initially dispersed Co atoms exist as Co-O4 units on the surface of the Au nanoparticle, where the Co-O4 exhibits relatively weak interactions with Au. Upon a potential of −0.8 V vs. RHE applied, Co1Ox@Au SAA undergoes reduction, resulting in a decreased Co-O coordination number and allowing more Co atoms to coordinate with Au to form Co1Au SAA, which in turn significantly strengthens the Co-Au interaction. Specifically, some Co atoms embed themselves into the surface of the nanoparticle, while others diffuse deeper into the interior, leading to increased interactions between Co and Au. This structural evolution culminates in the formation of a highly active Co1Au, optimizing the geometric and electronic configurations. These changes promote more favorable interactions with *COOH and *CO intermediates, as illustrated in FIG. 4(d), thereby enhancing the catalytic performance of the Au nanoparticles for the CO2RR.
-
In summary, utilizing multiple operando spectroscopic techniques, we successfully unraveled the surface structural evolution of the Co1Ox@Au SAA, establishing a direct link between its atomic configuration and catalytic performance in CO2RR. Operando SR-FTIR monitored the surface intermediates, revealing their relationship to the evolution of the active site. Operando XAS analysis further revealed that initially oxidized Co single atoms are gradually reduced and incorporated into the Au nanoparticle lattice under electrochemical conditions, resulting in enhanced Co-Au interactions within the lattice. This bimetallic interaction ensures an impressive CO selectivity of 92.2%. This study provides a comprehensive understanding of the atomic-scale structure-performance relationship of Co1Ox@Au and offers valuable strategic insights for designing efficient catalysts towards CO2RR.
Supplementary materials: The test details of the operando SR-FTIR spectra (including experimental setup, resolution, and data processing) are provided in the experimental section, along with detailed synthesis protocols, material characterization methods, electrochemical measurement procedures, operando XAS analysis, EXAFS fitting strategies, and supplementary figures (FIGs. S1–S4) and tables (Tables S1, S2).
Uncovering Self-Optimization of Single-Atom Alloy for Active CO2 Electrochemical Reduction Reaction
- Received Date: 14/09/2024
- Available Online: 27/04/2026
-
Key words:
- CO2 electrochemical reduction reaction /
- Electrocatalysis /
- Single-atom alloy /
- Operando X-ray absorption spectroscopy /
- Operando synchrotron-radiation Fourier transform infrared spectroscopy
Abstract: Renewable electricity-driven CO evolution from CO2 offers a promising route for sustainable chemical production. Single-atom alloy (SAA) catalysts are emerging as promising candidates for electrochemical CO2 reduction. However, the dynamic nature of SAAs within their local microenvironment often complicates our understanding of the underlying mechanisms that contribute to their enhanced performance. In this study, we introduce a single-atom Co-modified Au nanoparticle catalyst (Co1Ox@Au) for the electrocatalytic reduction of CO2 to CO. Using operando X-ray absorption spectroscopy (XAS), we observe the dynamic transformation of Co1Ox@Au into a low-valence Co1Au SAA, driven by the applied voltages. This behavior strengthens the atomic interaction between Au and Co, thus ensuring a reinforced adsorption of the crucial *COOH intermediate, which is corroborated by operando synchrotron-radiation Fourier transform infrared spectroscopy (SR-FTIR). Furthermore, the strengthened Au-Co interaction facilitates the subsequent desorption of the *CO intermediate, allowing for efficient CO formation and release. These insights highlight the self-optimization behavior of SAAs towards improving CO2 reduction selectivity.