In contrast to the inert properties in bulk [1], gold nanoparticles supported on metal oxides, especially TiO2, present efficient catalytic activities for acetylene hydrochlorination [2, 3], CO oxidation [4−6], water gas shift reaction [7, 8], as well as hydrogenation of aldehydes and unsaturated hydrocarbons [9, 10], etc. Great efforts have been exerted on understanding the origin of the unique activities of Au nanoparticles [11−13], which is important in the developments of gold catalysts with high catalytic performances and the large-scale industrial applications. A large number of publications describe the link of catalytic activity to the roles of electronic structures of Au nanoparticles, uncoordinated Au atoms, supports, perimeter sites, defects, and impurities [4, 8, 10, 11].
The study of CO adsorption on Au nanoparticles is of great significance not only for the industrial applications but also for the conceptual understanding of Au catalysis. The stretching vibration mode of CO molecule exhibits a high absorption coefficient of infrared light and an accurate response to the geometric morphology and electronic structure of catalysts [14], which can be used to characterize the chemical environment and valence states of Au particles. Thus, it is commonly used as a probe molecule in the infrared (IR) spectroscopy study of Au catalysts [15]. The IR peak of Au0–CO on the metallic Au (Au0) is generally located at 2110–2100 cm−1 [13, 16−19]. If the Au bears a slight positive charge, the vibration of CO blueshifts to 2130–2110 cm−1 which is attributed to the Auδ+–CO (0<δ<1) [18−21]. The signal appearing above 2140 cm−1 is considered to originate from CO adsorbed on Au+ or Au3+ [22]. Numerous studies suggest that the signal of 2090–2000 cm−1 stems from CO adsorbed on the negatively charged Au [16, 21, 23−25].
However, metals or supports are sometimes subject to structural or oxidation state alterations when exposed to CO atmospheres [26]. For example, Wang et al. [27] have reported the formation and migration of Au-CO complexes on Au(111). Jugnet et al. [28] revealed that 1–100 Torr CO induces a profound reorganization of the Au(110)(1×2) surface by STM. The size-dependent order-to-disorder transformation of Au particles on CeO2 upon CO exposure has been observed using environmental transmission electron microscopy (ETEM) [29]. Yuan et al. [12] observed a ~10° rotation of gold nanoparticles during CO oxidation and reverted to their initial positions after CO removal. Besides, CO can also influence the valence state of the support. Oxygen vacancies can be generated at the Au/TiO2 perimeter interface by the reaction between CO and lattice oxygen [30−32]. The spreading of Au particles and charge transfer from the reduced TiO2 to Au were evidenced by the appearance of a low frequency of C–O vibration at 2060 cm−1 [32].
The dynamic changes of metals and supports under CO atmosphere, combined with the unintended impurities during experiments, sometimes complicate the attribution of CO species on Au/TiO2. It has been reported that volatile impurities of Ni carbonyls can easily form by the reaction of CO with Ni, which is an extensive element in the stainless-steel gas cylinders/chambers [33−35]. Recent experiments showed that the unintended Ni carbonyl compounds can dissociate on the catalyst surface, thereby exerting an impact on the adsorption of CO on the metal [34, 35]. The above findings caution that neglecting the presence of Ni contamination in CO may result in the misattribution of IR peaks and consequently affect the comprehension of the catalytic mechanism. In this study, we systematically investigated the CO adsorption behavior of Au nanoparticles supported on TiO2 and identified the size effect of Au nanoparticles under the influence of Ni contamination.
-
The Au/TiO2 catalyst was prepared by the deposition-precipitation method [23]. 1 g of anatase TiO2 powder was added into 40 mL of 12.6 mmol/L HAuCl4 solution with the pH being maintained at 9.0 by adding 0.1 mol/L NaOH. The above-prepared suspension was heated to 65 °C and kept for 1 h. Then the Au/TiO2 solids were separated after centrifugal washing for several times and dried at 60 °C overnight. The obtained Au/TiO2 powders were then calcined at 250 °C for 2 h in air atmosphere (denoted as Au/TiO2-250). The gold concentration was 10.5 wt.% measured by inductively coupled plasma-mass spectrometry (ICP-MS) method. The above-prepared Au/TiO2-250 sample was annealed at 500 °C for 4 h to obtain Au/TiO2-500 sample with larger Au particles.
-
The Au-Ni/TiO2 catalyst was prepared using the deposition-precipitation method with urea [9]. 1 g of anatase TiO2 was dried at 100 °C for 24 h, then mixed with 60 mL of 4.2 mmol/L HAuCl4, 0.075 g of Ni(NO3)3·6H2O, 1.5 g of urea under stirring. The mixture was maintained at 80 °C for 16 h. Afterwards, the product was centrifuged and washed for several times, dried overnight, and finally reduced at 300 °C in the gas mixture of 10% H2 and 90% Ar for 2 h.
-
The surface morphology of Au/TiO2 powders was characterized by field emission transmission electron microscope (FE-TEM, JEM-2100F). The X-ray diffraction (XRD) data were collected using a Rigaku Smart Lab diffractometer with Cu Kα radiation. The X-ray photoelectron spectra (XPS) were collected on a Thermo ESCALAB 250Xi spectrometer with a monochromatized Al Kα excitation source (hν = 1486.6 eV).
Diffuse reflectance infrared Fourier transform spectroscope (DRIFTS) investigations were performed in a Harrick PRAYING MANTIS reaction chamber coupled to a Nicolet iS50 spectrometer equipped with a liquid nitrogen-cooled MCT detector. A spectral resolution of 4 cm−1 was used to collect the spectra, which were reported in Kubelka−Munk (K−M) units. Before each IR adsorption experiment, the sample was pretreated under 20 Torr O2 at 473 K for 30 min in the IR chamber. Then O2 was evacuated, and the sample was cooled down to room temperature in vacuum. The IR spectrum collected under vacuum conditions after pretreatment was used as the background spectrum, and each reported spectrum was an average of 64 scans. The difference spectra were collected at different CO pressures, with the number of scans for each difference spectrum set to 16.
-
FIG. 1 (a) and (b) show the transmission electron microscopy (TEM) images of Au/TiO2-250 and Au/TiO2-500, respectively. The insets display that the average particle size of Au is approximately 2.8 nm for Au/TiO2-250 sample and 6.6 nm for Au/TiO2-500 sample after calcination. The characteristic peaks of Au 4f7/2 on both Au/TiO2-250 and Au/TiO2-500 samples in FIG. 1(c) are located at 83.3 eV, indicating that Au has been successfully loaded on the TiO2 surface and exists in the zero-valent state [36]. FIG. 1(d) shows the XRD patterns of Au/TiO2 samples. No obvious Au diffraction peaks are observed on Au/TiO2-250 due to the small size of Au particles [37]. On Au/TiO2-500, a small peak of Au(200) appears at 44.4° and the strongest peak Au(111) at 38.2° overlaps with the peak of TiO2.
FIG. 2(a) and FIG. S1(a) in Supplementary materials (SM) show the time-evolved IR spectra of 10 Torr CO exposed to the fresh Au/TiO2-250 powders over a period of 10 min. A vibrational peak at 2109 cm−1 emerges and reaches the maximum intensity in 2 min, and then the peak position shifts to 2105 cm−1. This peak is attributed to the C–O stretching vibrational mode of CO adsorbed on the metallic Au nanoparticles [13, 16−19]. The single narrow peak indicates homogeneous adsorption sites on the Au particle. As shown in FIG. S1(b) (SM), the CO peak intensity gradually declines and the peak position shifts back to a higher frequency as the equilibrium CO pressure decreases. The complete disappearance of CO peak upon evacuation indicates that CO adsorption on Au is reversible under the experimental conditions.
The observed redshift of CO vibrational frequency at high CO coverage (insets in FIG. S1(a, b) of SM) can be rationalized through the Blyholder model [38]. The Au–CO bond is primarily formed through the electron donation from the 5σ orbital of CO to Au and the limited backdonation from the deep-lying d orbitals of Au to the 2π
$ ^* $ antibonding orbital of CO. As the CO coverage increases, the electron density on Au particles increases and thus decreases the extent of the donation of electrons from the 5σ orbital to Au, which results in the destabilization of C–O bond and thus the redshift of the CO vibration frequency [39].In addition to the 2105 cm−1 peak, a secondary peak at 2050 cm−1 (FIG. 2(b) and FIG. S2 in SM) is observed on the Au/TiO2-250 sample after multiple CO exposure experiments (denoted as Au/TiO2-250-aged). FIG. 2(b) shows the time-evolved IR spectra of CO adsorbed on the Au/TiO2-250-aged sample. The temporal variations of the peak intensities and peak positions of the two peaks at 2105 cm−1 and 2050 cm−1 are shown in FIG. 2(c, d). The 2105 cm−1 peak emerges at 0.1 min and quickly reaches saturation at ~1 min after CO exposure, whereas the 2050 cm−1 peak intensity gradually increases over time. Furthermore, the 2105 cm−1 peak undergoes redshift, while the 2050 cm−1 exhibits a blueshift.
There are several possible explanations for the origin of the peak at ~2050 cm−1. In many reports, a peak located below 2090 cm−1 was attributed to CO adsorbed on the supported negatively charged Au particles (Auδ––CO) [16, 21, 23−25]. The reduction of Au0 to Auδ– may occur via CO or electron transfer from the reduced support to Au [24]. Roze et al. [25] demonstrated that the surface of Au would undergo reconstruction, forming new Au adsorption sites and generating an IR band at 2070 cm−1. Recently, Yao et al. [34] proposed that the vibrational peak ranging from 2090 cm−1 to 1900 cm−1 on the Au surface is from the adsorption of CO on the Ni impurity caused by the dissociation of Ni(CO)4 in the CO gas on Au nanoparticles. Ni(CO)4 comes from the reaction of CO with Ni under high pressure and becomes the unintended contamination in CO gas [33−35]. FIG. S3 in SM shows the Ni 2p XPS spectra of the Au/TiO2-250 and Au/TiO2-250-aged samples. In contrast to the Au/TiO2-250 sample, a broad spectral envelope appears in the 850–870 eV region, and no distinct Ni peaks can be distinguished. This is likely due to the trace amount of Ni below the detection limit of XPS.
The melting point of Ni(CO)4 is 253.9 K and the boiling point is 315.4 K [40], which can be easily removed when CO gas passes through the liquid nitrogen cold trap. To verify the origin of the 2050 cm−1 peak, a liquid nitrogen cold trap was employed to remove the nickel-carbonyl impurities from the CO gas, and further experiments were conducted with the results shown in FIG. 3. In FIG. 3(a), 10 Torr CO was exposed to the fresh Au/TiO2-250 powder (black curve), and Au/TiO2-250 powders subject to 760 Torr purified (red curve) and unpurified CO (blue curve) exposures for 10 min. A vibrational peak at 2105 cm−1 is observed on all the samples, while the 2050 cm−1 peak appears exclusively on the unpurified CO-exposed Au/TiO2-250 sample. This clearly demonstrates that the 2050 cm−1 peak originates from Ni contaminants from the stainless-steel gas cylinders instead of restructuring or reduction of Au subject to high CO exposure.
To further confirm the adsorption behavior of Ni, Au-Ni alloy clusters with a size of ~3.1 nm supported on anatase TiO2 surfaces were prepared and the adsorption of CO (FIG. S4 in SM) was investigated. FIG. 3(b) shows the time-evolved infrared spectra of the purified 10 Torr CO adsorbed on the Au-Ni/TiO2 powder from 0 to 10 min. In addition to the rapidly saturated Au–CO vibrational peak at 2100 cm−1, the Ni–CO peak at 2045 cm−1 is also observed. The peak intensity of the Ni–CO gradually increases within 0–10 min, and the peak position undergoes a blueshift as the coverage increases, which is consistent with the observations in FIG. 2. This further confirms that the 2050 cm−1 peak in FIG. 2 originates from Ni contamination in the CO gas.
The increase in the intensity of the Ni-CO vibrational peaks with exposure time in FIG. 2(b) and FIG. 3(b) can be explained by the gradual segregation of Ni towards the Au surface. DFT calculations indicated that Ni atoms are energetically stable on the surface of Au in CO atmosphere [41] and favor the subsurface layer of Au under vacuum conditions [42]. Therefore, we propose that Ni contaminants formed by the dissociation of Ni(CO)4 enter the subsurface/bulk of the Au particles under vacuum, and under a CO atmosphere, the bulk Ni atoms progressively segregate towards the Au surface, manifesting as an increasing signal in the infrared spectrum. The redshift of the frequency of the Ni-CO with increasing CO coverages results from the dipole-dipole interactions between adjacent CO molecules on Ni [43].
The apparent activation energy of Ni segregation under CO exposure can be determined from the Arrhenius equation. FIG. 4(a) shows the time-evolved infrared spectra of CO adsorption at 5 Torr for 10 min at 303 K, 308 K, 313 K, and 318 K on the Au/TiO2-250-aged sample. The integrated peak area of 2050 cm−1 (Ni–CO) at different temperatures versus CO exposure time was plotted in FIG. 4(b). A rapid initial increase in the first 100 s is independent of temperature and may correspond to the spillover of CO from the Au to the Ni sites and the formation of Ni-CO. The data points from 100 s to 600 s in FIG. 4(b) are linearly fitted to obtain the slope of the change of Ni–CO peak area over time, i.e., the rate (r) of Ni segregation to the surface at different temperatures. Then the apparent activation energy can be calculated from the Arrhenius plot in FIG. 4(c). The y-axis in FIG. 4(c) represents the natural logarithm of the reaction rate, and the x-axis represents the reciprocal of temperature. The same procedure was performed for 10 Torr and 15 Torr CO, as shown in FIG. S5 (SM). The apparent activation energy (Ea) under different CO pressures is 32.3 kJ/mol, 36.0 kJ/mol, and 42.6 kJ/mol at 5, 10, and 15 Torr, respectively.
The increase of the apparent activation energy for Ni segregation with increasing CO pressure can be tentatively explained by the Ni diffusion mechanism. It has been reported [44, 45] that the vacancies on Au enable atoms to move from one location to another and serve as channels for Ni atom diffusion. The presence of CO on Au stabilizes the vacancies in Au particles. Consequently, the apparent activation energy for the diffusion of Ni in Au particles also increases with increasing CO pressure.
Quantitative analysis of CO adsorption enthalpy on Au/TiO2-250 was conducted by IR in FIG. S6 (SM) and FIG. 5(a–c). FIG. 5(a) shows the adsorption isotherms of CO on Au/TiO2-250 at various temperatures. The linear relationship between the logarithm of pressure (p) and the reciprocal of temperature (T) at different IR peak areas (corresponding to different CO coverages) is shown in FIG. 5(b). Based on the Clausius-Clapeyron equation,
the adsorption enthalpy (ΔH) corresponding to different CO coverages is obtained, ranging from −39.0 kJ/mol (peak area of 0.8) to −44.1 kJ/mol (peak area of 0.3) in FIG. 5(c), which is close to the previously reported value by Goodman et al. [17]. The decrease of the adsorption enthalpy as a function of the CO coverage can be explained by the weakening of Au–CO bond due to the decrease in the extent of the donation of electrons from the 5σ orbital to Au at higher CO coverage, as discussed in FIG. 2 [39].
The influence of Ni on the adsorption enthalpy of CO on Au was systematically investigated in FIG. S7 (SM) and FIG. 5(d, e). FIG. 5(d) shows the adsorption isotherms of CO at different temperatures on Au/TiO2-250-aged nanoparticles. FIG. 5(e) depicts the relationship between the logarithm of pressure and the reciprocal of temperature on the Au/TiO2-250-aged surface, revealing that the linear relationship remains unaffected by the presence of Ni contamination. FIG. 5(f) shows the adsorption enthalpies of Ni-contaminated Au/TiO2-250 surfaces under different Au–CO peak areas. As the Au–CO peak area increases, the adsorption enthalpy decreases, ranging from −22.2 kJ/mol at a peak area of 1.4 kJ/mol to −26.9 kJ/mol at a peak area of 0.4. The significant reduction in the absolute value of the adsorption enthalpy compared to the uncontaminated surface may be attributed to the electron transfer from Ni to Au, weakening the interaction between CO and Au. FIG. S8 (SM) shows the Au 4f XPS spectra of the Au/TiO2-250 and Au/TiO2-250-aged samples. In the Au/TiO2-250 sample, the Au 4f7/2 peak is located at 83.3 eV. Compared with the fresh sample, the Au 4f7/2 peak (83.2 eV) in the Ni-contaminated sample shifts by 0.1 eV toward lower binding energy, indicating electron transfer from Ni to Au.
To investigate the influence of Au size on Ni contamination, FIG. 6 (a) and (b) show the time-evolved IR spectra of 10 Torr CO adsorbed on the Au/TiO2-500 with an Au size of 6.6 nm and the Au/TiO2-500-aged (Au/TiO2-500 sample after multiple CO exposure experiments) respectively. In FIG. 6(a), a vibrational peak located at 2100 cm−1 is observed besides the gas-phase CO peak. However, a new peak at 2030 cm−1 appeared in FIG. 6(b) alongside 2100 cm−1 CO mode. This is consistent with the result in FIG. 3, which indicates that that the peak around 2050 cm−1 originates from Ni contamination in the CO rather than from CO adsorbed on smaller Au clusters or Auδ−. However, the 2030 cm−1 peak on the Au/TiO2-500-aged quickly saturated within a short time and did not change over time.
The distinct CO adsorption behaviors on Ni contaminated Au/TiO2-250 and Au/TiO2-500 can be attributed to the size effect of Au. On the Au/TiO2-500, Ni impurities cannot diffuse into the bulk of Au to form Ni-Au alloys and instead tend to aggregate into Ni clusters either on the TiO2 or Au surface. As a result, upon CO exposure, the Ni–CO peak rapidly saturates and no segregation can be observed. This is supported by the TEM experiments by Bogatyrenko et al. [46], who found that bulk-immiscible Au and Ni form a homogeneous solid solution after heating Au-Ni nanoparticles when the size decreases to approximately 2 nm at room temperature.
Meunier et al. [35] reported that Ni(CO)4 can dissociate not only on the surface of Au but also on Cu surfaces. Additionally, Zecchina and co-workers [47] observed that strong Lewis acid sites on alumina facilitate the slow decarbonylation of Ni(CO)4 at 50 °C. As a control experiment, the adsorption of unpurified CO with Ni contaminants was also investigated on the surface of anatase TiO2 powder (FIG. S9 in SM). No significant difference is observed on fresh TiO2 and TiO2 subjected to unpurified CO exposure. The absence of Ni-CO vibrational peak in FIG. S9 (SM) suggests that Ni(CO)4 does not decompose to form Ni impurities on the TiO2 surface without Au loading. Therefore, we conclude that the contaminated Ni originates from the dissociation of Ni(CO)4 in the CO gas on Au nanoparticles.
Based on the above discussion, FIG. 7 schematically illustrates the adsorption model of contaminated CO on the Au/TiO2 nanoparticles of different sizes. For the 2.8 nm Au/TiO2, Ni(CO)4 impurities in the CO atmosphere dissociate on the surface of Au particles, and Ni atoms incorporate into the bulk of Au forming alloys. Upon subsequent CO exposure, Ni segregates to the Au surface and bonds with CO. In contrast, for the 6.6 nm Au/TiO2, Ni contaminant remains on the surface of Au particles, and no significant bulk diffusion occurs.
-
In summary, this study sets out to explore the influence of Ni impurities on the CO adsorption on Au/TiO2 powders. On the 2.8 nm Au/TiO2, the volatile impurity Ni(CO)4 in the CO atmosphere dissociates on the surface of Au particles and diffuses into the bulk of Au. Upon subsequent CO exposure, Ni segregates from the bulk to the Au surface and bonds with CO, forming an IR peak at 2050 cm−1. The apparent activation energy for Ni segregation was measured to be 32.3 kJ/mol, 36.0 kJ/mol, and 42.6 kJ/mol under different CO pressures at 5, 10, and 15 Torr, respectively. Moreover, the adsorption enthalpy of CO on the Au/TiO2 decreases significantly in the presence of contaminated Ni due to the electron transfer from Ni to Au. The behavior of Ni contamination is affected by the size of Au. In contrast, on the 6.6 nm Au/TiO2, the Ni contaminant remains on the Au particle surface without diffusing into its bulk phase. These findings remind us of the important roles of unintended Ni impurities on the characterization of the catalytic behavior of Au/TiO2 in the presence of CO.
CO Adsorption Behavior on Au/TiO2 and Associated Size Effects Under the Influence of Ni Contamination
- Received Date: 01/05/2025
- Available Online: 27/10/2026
-
Key words:
- CO adsorption /
- Au/TiO2 /
- Infrared spectroscopy /
- Ni /
- Size effect
Abstract: The dynamic changes of metals and supports under CO atmosphere, combined with the potentially undetected Ni impurities, frequently complicate the attribution of CO species and lead to controversial mechanism interpretations in Au/TiO2 catalysis. The influence of Ni contamination on the CO adsorption by Au nanoparticles supported on TiO2 has been investigated by Fourier transform infrared spectroscopy. On the 2.8 nm Au nanoparticles, the impurity Ni(CO)4 in the CO atmosphere dissociates on the surface of Au particles and diffuses into the bulk of Au to form an alloy. Upon subsequent CO exposure, Ni segregates to the Au surface and bonds with CO. The apparent activation energy of ~37 kJ/mol for Ni segregation in the presence of CO was measured. The presence of Ni significantly decreases the adsorption enthalpy of CO on Au due to the electron transfer from Ni to Au. In contrast, on the 6.6 nm Au nanoparticles, the Ni contamination remains on the Au particle surface and no bulk phase penetration occurs. These findings highlight the critical yet often overlooked influence of trace Ni contamination when characterizing Au/TiO2 catalytic systems under CO atmosphere.