Wanyun Tang, Yuehui Luo, Can Zhu, Nan Huang, Quanxin Li. Selective Synthesis of Bio-based Benzaldehyde Using Magnetic CoFe2O4@Biochar(HTR) Catalyst†[J]. Chinese Journal of Chemical Physics, 2026, 39(1): 125-135. doi: 10.1063/1674-0068/cjcp2510165
Citation: Wanyun Tang, Yuehui Luo, Can Zhu, Nan Huang, Quanxin Li. Selective Synthesis of Bio-based Benzaldehyde Using Magnetic CoFe2O4@Biochar(HTR) Catalyst†[J]. Chinese Journal of Chemical Physics, 2026, 39(1): 125-135. doi: 10.1063/1674-0068/cjcp2510165

Selective Synthesis of Bio-based Benzaldehyde Using Magnetic CoFe2O4@Biochar(HTR) Catalyst†

  • Corresponding author: E-mail: liqx@ustc.edu.cn
  • Received Date: 23/10/2025
    Available Online: 27/02/2026
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(6)

Article Metrics

Article views(126) PDF downloads(0) Cited by(0)

Access History

Selective Synthesis of Bio-based Benzaldehyde Using Magnetic CoFe2O4@Biochar(HTR) Catalyst†

Abstract: Developing green and efficient methods to acquire lignocellulose-based chemicals with high added value is beneficial for facilitating green chemistry and sustainable development. The goal of this study is to demonstrate that bio-based benzaldehyde, a noteworthy high-value chemical, is able to be directionally prepared from lignocellulosic biomass. This new controllable transformation was materialized by uniting catalytic-pyrolysis of lignocellulose to toluene intermediate and catalytic oxidation of toluene intermediate to bio-based benzaldehyde. This work also developed a highly active magnetic catalyst (CoFe2O4@Biochar(HTR)), achieving 77.1% benzaldehyde selectivity and 46.7% benzaldehyde yield using this catalyst. It was found that introducing the biochar carrier into the cobalt iron composite metal oxide catalyst enhanced hydroxyl radical formation and bio-based benzaldehyde synthesis. Based on catalyst characterizations and hydroxyl radical analysis, potential reaction mechanism for bio-based benzaldehyde synthesis was proposed. This strategy may provide a beneficial pathway for developing high-value bio-based chemical (benzaldehyde) using renewable lignocellulosic biomass.

    • Lignocellulosic biomass is primarily composed of three core constituents (namely cellulose, hemicellulose, and lignin), regarded as a generous renewable resource [1, 2]. In lignocellulose, cellulose is a highly crystalline polymer, composed chiefly of glucose units [3]. Hemicellulose is an amorphous heterogeneous polymer, constructed by different monosaccharides such as xylose and arabinose [4]. Lignin is an amorphous aromatic polymer with a three-dimensional network structure, formed by three phenylpropane units (guaiacylpropane, syringaylpropane, and 4-hydroxyphenylpropane) [5]. Based on thermochemical or biochemical conversion ways, various high-value chemicals can be produced from lignocellulosic biomass, including ethanol, butanol, polyols, furan compounds, aromatic aldehydes, and aromatic acids [1, 2, 6, 7].

      Benzaldehyde is one of the most important aromatic aldehydes in industry, widely adopted for manufacturing pharmaceuticals, spices, dyes as well as lubricants [8]. At present, there are two main industrial processes for producing benzaldehyde from toluene, including toluene chlorination-hydrolysis and toluene homogeneous oxidation [8, 9]. The toluene chlorination-hydrolysis process mainly includes three steps: chlorination of toluene to form benzyl chloride intermediate, acid hydrolysis of intermediate to form the mixed products (benzyl alcohol, benzaldehyde, and benzoic acid), and distillation separation of the mixture to produce benzaldehyde [8, 9]. The homogeneous oxidation process of toluene can produce the main product of benzoic acid with the by-product of benzaldehyde, usually using cobalt acetate/manganese acetate as catalyst and halide as initiator [8, 9]. However, the main disadvantage of the above industrial processes is that they require very harsh reaction conditions and generate toxic waste, which is harmful to the environment and leads to equipment corrosion [8, 9].

      In the past decade, developing green processes for toluene oxidation to benzaldehyde has received increasing attention [8−16]. Early research mainly focused on homogeneous catalytic oxidation process of toluene using organic acid salts containing cobalt or manganese as catalysts [8, 10]. The main product obtained from the homogeneous catalytic oxidation of toluene was benzoic acid, and yet benzaldehyde yield was not high [8, 10]. Heterogeneous catalytic oxidation overcomes the difficulty of catalyst recovery in homogeneous catalytic oxidation process [8]. For the heterogeneous catalytic oxidation of toluene, precious metal catalysts often exhibit high selectivity to benzaldehyde [8, 11]. So far, heterogeneous catalytic oxidation of toluene using non-noble metal catalysts has received increasing attention [12−16]. Liu et al. reported that CoZrPWO immobilized zeolite catalyst had 90% benzaldehyde selectivity, but the toluene conversion was only 16.6% in the oxidation of toluene [12]. Zhang et al. reported a high benzaldehyde production rate of 4049 μmol·g−1h−1 when using N-hydroxyphthalimide (NHPI) and CoMnAl oxide co-catalysts [13]. Sutradhar et al. reported catalytic oxidation of toluene using Cu(II) complex as a catalyst, obtaining the maximum benzaldehyde yield of 11% [14]. Singha et al. reported the WO3 nanocube material had good photocatalytic oxidation activity of toluene to benzaldehyde, achieving a 79.3% benzaldehyde selectivity [15]. Xu et al. reported toluene oxidation to benzaldehyde catalyzed by CuCr bimetallic oxide catalyst, achieving the highest benzaldehyde yield of 42.9% [16]. However, benzaldehyde is an intermediate product in the oxidation of toluene, which can be further oxidized to form benzoic acid or other by-products [8]. Controlling the depth of oxidation is a key challenge in the synthesis of benzaldehyde [8]. Therefore, it is necessary to further explore heterogeneous catalysts and green reaction processes to efficiently synthesize benzaldehyde.

      So far, direct conversion of lignocellulosic biomass into benzaldehyde remains a highly challenging task, as the intermediates and products involved in biomass conversion are often very complex [7]. Here, we adopted a new approach for preparing bio-benzaldehyde based on uniting biomass catalytic pyrolysis and toluene oxidation. This work also developed a highly active and recyclable magnetic catalyst (CoFe2O4@ Biochar(HTR)), which is suitable for the selective synthesis of benzaldehyde. Based on catalyst characterization and hydroxyl radical analysis, a probable reaction mechanism for bio-based benzaldehyde synthesis was proposed. This strategy may provide a beneficial pathway for producing high value benzaldehyde chemical using renewable biomass.

    II.   EXPERIMENTS
    • Straw powder, a typical lignocellulosic biomass, was obtained from Gaotang Agricultural Products Co., Ltd. (Shandong, China) [17]. The main element contents in the straw biomass were 48.22 wt% C, 6.25 wt% H, 0.67 wt% N, and 44.86 wt% O, which were measured by Elemental Analyzer (Vario EL cube, Elementar, Langenselbold, Germany). Cobalt-chloride (CoCl2·6H2O), ferric-chloride (FeCl3·6H2O), ethylene glycol and other commonly used reagents were obtained from Shanghai Aladdin Bio-Chem Technology Co., LTD (Shanghai, China).

    • The CoFe2O4(CO) catalyst was prepared by co-precipitation method [18]. First, FeCl3·6H2O (10 mmol) and CoCl2·6H2O (5 mmol) were dissolved into 50 mL deionized water under a constant magnetic stirring. Then, 1.0 mol/L NaOH (20 mL) was appended to the mixture and stirred at 90 °C for 2 h. The dried precipitate was calcined at 600 °C for 5 h, which was marked as CoFe2O4(CO) catalyst.

      The CoFe2O4(HTR) catalyst was synthesized via a modified hydrothermal route using ethylene glycol reducing agent [19]. First, 2.5 mmol CoCl2·6H2O and 5 mmol FeCl3·6H2O were dissolved in ethylene glycol solvent (40 mL). Then, polyethylene glycol (1.0 g) as well as sodium acetate (3.0 g) was appended to the mixed solution and stirred for one hour to obtain a suspension. Finally, the suspension was placed to a Teflon-lined autoclave and reacted at 200 °C for 20 h. The resulting solid sample was marked as CoFe2O4(HTR) catalyst. The CoFe2O4(HT) catalyst was prepared by a similar hydrothermal method without adding ethylene glycol reducing agent.

      The CoFe2O4@Biochar(HTR) catalyst was obtained based on a modified hydrothermal method using ethylene glycol as reducing agent and biochar as the support [17]. Biochar was obtained as a solid by-product of straw catalytic pyrolysis [20]. Firstly, dried biochar (1.0 g) was dispersed in ethylene glycol solvent (10 mL), which was labelled as “Solution A”. Separately, 2.0 mmol CoCl2·6H2O and 4.0 mmol FeCl3·6H2O were dispersed in ethylene glycol solvent (30 mL), which was labelled as “Solution B”. Then, sodium acetate (3.0 g), polyethylene glycol (1.0 g) as well as “Solution A” were added to “Solution B” and stirred for one hour to get a uniform suspension. Finally, the mixture was placed in a Teflon-lined autoclave and reacted at 200 °C for 20 h. The dried solid sample was marked as CoFe2O4@Biochar(HTR) catalyst. Typically, the CoFe2O4@Biochar(HTR) catalyst contained 35.2 wt% CoFe2O4 (active component) and 64.8 wt% Biochar (catalyst support), which were determined by thermo-gravimetric analysis (TGA) using a Mettleroledo TGA/DTA-851e analyzer (Mettleroledo Co., Bern, Switzerland).

    • The crystalline phases of catalysts were probed via an X-ray diffraction equipment (SmartLab SE, Rigaku Corporation, Tokyo, Japan) [17]. X-ray photoelectron spectroscopy (K-Alpha, Thermo Fisher Scientific, Waltham, MA, USA) was adopted to analyze elemental chemical states in catalysts [18]. Functional groups of catalysts were characterized via a Nicolet IS10 FTIR equipment (Fourier transform infrared spectroscopy, Thermo Fisher Scientific, Waltham, MA, USA) [21]. Morphology of catalysts were examined by scanning electron microscopy (SEM, Gemini 300, Carl Zeiss AG, Oberkochen, Germany) [22]. Oxygen vacancies in the catalysts were probed using an electron paramagnetic resonance spectrometer (EPR, JES-FA 200, JEOL Ltd., Tokyo, Japan) [23]. Magnetic properties of the catalysts were examined via a vibrating sample magnetometer (VSM, 8604, Lake Shore Cryotronics, Inc., Westerville, OH, USA) [23]. Metal ion leaching during catalytic tests was quantified by inductively coupled plasma atomic emission spectrometer (ICP-AES, ICP 7400, Thermo Fisher Scientific, Waltham, MA, USA) [24].

    • In this study, an aromatic intermediate, predominantly toluene, was used as the substrate for bio-based cresol synthesis. The aromatic intermediate was obtained via catalytic pyrolysis of straw biomass using 5%Zn@HZSM-5 catalyst, following our previously reported procedure [20]. As present in Table S1 (see Supplementary materials (SM)), crude aromatic intermediate contained primarily toluene alongside lower-content aromatics (benzene, xylene, trimethylbenzene, naphthalenes, and indenes). To enhance benzaldehyde’s selectivity, crude aromatic intermediate was pretreated by distillation. The pretreated aromatic intermediate was mainly composed of 90.4 wt% toluene, 5.6 wt% benzene, and 2.2 wt% xylenes (Table S1 in SM). Considering that we have conducted in-depth research on preparing aromatic intermediates via biomass catalytic pyrolysis in our previous work [20, 25], this study concentrates on catalytic oxidation of aromatic intermediate.

      The catalytic oxidation of aromatic intermediate (rich in toluene) was carried out using different Co-Fe composite metal oxides. The bio-benzaldehyde synthesis was conducted in a 25 mL reactor, typically containing 2.0 g of substrate, 4.0 g of acetonitrile solvent, and 0.2 g of catalyst. A 30 wt% hydrogen peroxide (6 mL) solution was served as the green oxidation reagent. Upon reaction completion, magnetic catalysts were recovered from the products with an external magnet, and liquid products were quantitatively measured via a GC-MS (Thermo-Trace GC/ISQ MS, Thermo-Fisher Scientific, USA). The conversion, product’s yield and selectivity were evaluated following our previous work [25]. In addition, hydroxyl radicals formed in catalytic oxidation using different Co-Fe composite catalysts were probed by EPR analysis (JES-FA 200, JEOL Ltd., Tokyo, Japan) [25].

    III.   RESULTS AND DISCUSSION
    • FIG. 1(a) presents XRD patterns of Co-Fe composite catalysts. CoFe2O4(CO) catalyst synthesized by co-precipitation method shows characteristic diffraction peaks at 18.3°, 30.1°, 35.4°, 43.1°, 53.5°, 57.1°, 62.6°, and 74.0°, assigned to (111), (220), (311), (400), (422), (511), (440), and (533) planes of CoFe2O4 nanoparticle [26]. The CoFe2O4(HT) and CoFe2O4(HTR) catalysts were synthesized using hydrothermal method without and with ethylene glycol reductant, respectively. The XRD patterns of the CoFe2O4(HT) and CoFe2O4 (HTR) catalysts were consistent with that of the CoFe2O4(CO) catalyst. The CoFe2O4@Biochar(HTR) catalyst was synthesized via the hydrothermal method with ethylene glycol reducing agent and biochar support. The biochar supporter shows two wide profile peaks centered at 23.8° and 44.0°, assigned to (002) and (100) planes of graphitic carbon, respectively [27]. The CoFe2O4@Biochar(HTR) catalyst shows diffraction peaks of two components: CoFe2O4 nanoparticle and biochar support (FIG. 1(a)).

      FIG. 1(b) presents FTIR spectra of the Co-Fe composite catalysts. The CoFe2O4(CO) catalyst shows four absorption peaks at 3442, 1630, 590 and 420 cm−1, assigned to O−H stretching mode, H−O−H bending mode (absorbed water), Fe−O stretching mode and Co−O stretching mode (in CoFe2O4), respectively [26]. FTIR spectra of the CoFe2O4(HT) and CoFe2O4 (HTR) catalysts are basically the same as that of the CoFe2O4(CO) catalyst. The biochar carrier shows absorption peaks near 3442, 1698, 1592, 1420, 1160, 872 cm−1, assigned to O−H stretching mode, C=O stretching mode, C=C stretching mode, H−C−H bending mode, C−O stretching mode, and aromatic C−H out-of-plane bending mode, respectively [27]. CoFe2O4@Biochar(HTR) catalyst shows characteristic absorption peaks of CoFe2O4 and biochar carrier.

      FIG. 2(a) presents XPS full-survey spectra of Co-Fe composite catalysts. Based on XPS analysis, CoFe2O4(CO), CoFe2O4(HT) and CoFe2O4(HTR) catalysts contain Co, Fe, and O elements. The CoFe2O4@Biochar(HTR) catalyst contains four elements of Co, Fe, O, and C. FIG. 2(b) presents Fe 2p spectra of different catalysts. To help the identification, Fe 2p spectra of Fe2O3 and Fe3O4 were also analyzed. Similar to Fe2O3 catalyst, CoFe2O4(HT) catalyst shows four peaks near 710.8, 718.8, 724.3, and 732.5 eV, assigned to the main peak of Fe3+ 2p3/2, its satellite peak, the main peak of Fe3+ 2p1/2, and its satellite peak, respectively [28]. The asymmetric Fe 2p3/2 peak can be well decomposed into two components near 710.8 and 713.5 eV, assigned to Fe3+ species in octahedral sites (Fe3+(Oh)) and tetrahedral site (Fe3+(Td)) respectively [28]. The chemical state of Fe in the CoFe2O4(CO) catalyst also appeared as trivalent iron (Fe3+). Similar to the Fe3O4 catalyst, Fe 2p3/2 peak of CoFe2O4(HTR) catalyst can be well decomposed into three components around 709.9, 710.8, and 713.5 eV, assigned to Fe2+(Oh), Fe3+(Oh) and Fe3+(Td) respectively [28]. The Fe2+ species in the CoFe2O4(HTR) catalyst was attributed to the reduction of some Fe3+ species by ethylene glycol reductant [29]. The Fe2+/Fe3+ ratio for the CoFe2O4@Biochar(HTR) catalyst was 0.78, higher than the ratio value of the CoFe2O4(HTR) catalyst (0.65). This indicated that the addition of biochar carrier to the CoFe2O4(HTR) catalyst promoted the reduction of Fe3+ to Fe2+ [30].

      As present in FIG. 2(c), Co 2p spectra of all Co-Fe composite catalysts are similar to that of CoO catalyst. All Co 2p spectra show four peaks near 780.1, 785.2, 795.6, and 802.2 eV, assigned to the main peak of Co2+ 2p3/2, its satellite peak, the main peak of Co2+ 2p1/2, and its satellite peak, respectively [26]. The Co 2p XPS results confirm that the chemical state of Co in the Co-Fe composite catalysts belongs to divalent cobalt ion (Co2+), consistent with previous work [26]. Similar to CoO catalyst (FIG. 2(d)), O 1s spectra of CoFe2O4(CO) and CoFe2O4(HT) catalysts can be well deconvoluted into lattice oxygen and physically adsorbed oxygen, in agreement with previous work [31]. O 1s spectrum of CoFe2O4(HTR) catalyst can be well deconvoluted into three bands near 529.8, 531.1, and 531.8 eV, assigned to lattice oxygen (Olat), oxygen vacancies (Ov), and physically adsorbed oxygen (Oabs), respectively [31]. O 1s spectrum of biochar can be well deconvoluted into three bands near 531.5, 532.4 and 533.6 eV, assigned to C=O, C−O, and O−C=O bonds in biochar respectively [26]. Considering the contributions of two components (CoFe2O4 and biochar), O 1s spectrum of CoFe2O4@Biochar(HTR) catalyst can be well deconvoluted into five bands near 529.8, 531.1, 531.8, 532.4, and 533.6 eV, assigned to lattice oxygen (Olat), oxygen vacancies (Ov), C=O, C−O and O−C=O bonds in biochar respectively [26, 30]. The above results indicated that the addition of ethylene glycol reducing agent during the preparation of the catalysts can promote the formation of oxygen vacancies.

      FIG. 3 presents SEM images of Co-Fe composite catalysts. CoFe2O4(CO) catalyst exhibits serious particle aggregation, which may be caused by high-temperature sintering during the catalyst preparation process [31]. CoFe2O4(HT) catalyst, prepared by hydrothermal method, displays a series of spherical nano-particles (average diameter: ~158.1 nm). CoFe2O4(HTR) catalyst displays more dispersed spherical nano-particles (average diameter: ~142.2 nm). SEM image of the CoFe2O4@Biochar(HTR) catalyst shows that spherical particles are attached to the surface of biochar carrier. CoFe2O4@Biochar(HTR) catalyst shows a smaller average diameter (131.1 nm) than that of the CoFe2O4(HTR) catalyst (142.2 nm). The above results inferred that introducing biochar carrier into CoFe2O4 catalyst dispersed the active component (CoFe2O4) and reduces particle aggregation.

      To further confirm oxygen vacancies, EPR analysis has been conducted for different catalysts (FIG. 4(a)). For CoFe2O4(CO) and CoFe2O4(HT) catalysts, no EPR signal was detected. However, CoFe2O4(HTR) catalyst shows a clear EPR signal (g=2.0030), assigned to oxygen vacancies (Ov) in the catalyst [32]. In addition, biochar carrier also exhibits a sharp EPR signal (g=2.0036), assigned to free radical species (aromatic radicals) in biochar [33]. The CoFe2O4@Biochar(HTR) catalyst shows a stronger EPR signal (g=2.0031) than the CoFe2O4(HTR) catalyst. The above EPR results are consistent with the XPS characterization results (FIG. 2(d)). As shown in FIG. 4(b), the magnetic property of the catalysts was investigated by measuring magnetic hysteresis loop [26]. The saturation magnetization of CoFe2O4(HT) catalyst was 70.0 emu/g, which is slightly stronger than CoFe2O4(CO) catalyst (67.0 emu/g). The saturation magnetization of CoFe2O4@Biochar(HTR) catalyst significantly decreased to 24.3 emu/g, indicating that the addition of non-magnetic biochar carrier dispersed the magnetic component (CoFe2O4). Nevertheless, CoFe2O4@Biochar(HTR) catalyst still retains sufficient magnetic property for the catalyst recovery by an external magnetic field (see image inserted in FIG. 4(b)).

    • In this work, we used pretreated aromatic intermediate to prepare bio-based benzaldehyde (Table S1 in SM). No detectable products were formed without a catalyst, as the self-dissociation of hydrogen peroxide cannot effectively generate hydroxyl radicals [17]. When the Co-Fe composite metal oxide catalysts were used, benzaldehyde was yielded via selective oxidation of toluene intermediate (Table S2 in SM). CoFe2O4(HTR) catalyst shows a higher benzaldehyde yield (41.7%) than the CoFe2O4(HT) catalyst (31.9%). According to XPS characterization (FIG. 2), the addition of ethylene glycol reducing agent during catalyst preparation can increase the Fe2+/Fe3+ ratio in the Co-Fe composite catalyst, which is beneficial for the formation of ·OH radicals [17]. As shown in Table S2 (SM), the CoFe2O4@Biochar(HTR) catalyst shows the highest benzaldehyde yield (46.7%) among the tested catalysts. The SEM characterization confirmed that the introduction of biochar support in the CoFe2O4 catalyst reduced particle aggregation and dispersed the active centers of the catalyst (FIG. 3). The XPS characterization verified that the introduction of biochar support in the catalyst increased the Fe2+/Fe3+ ratio, which is beneficial for ·OH radicals’ formation [17]. As a comparison, a single metal oxide catalyst (Co3O4) shows lower benzaldehyde yield than the CoFe2O4@Biochar(HTR) catalyst. When using the preferred CoFe2O4@Biochar(HTR) catalyst, the main product was benzaldehyde with a selectivity of 77.1% (Table S2 in SM), which was formed by side chain oxidation of toluene in aromatic intermediate. Besides, a small amount of by-products of benzoic acid came from benzaldehyde’s deep-oxidation, while toluene hydroxylation and cresol secondary oxidation give rise to forming by-products of cresol as well as methyl benzoquinone, respectively [20]. As shown in Table S1 (SM), the pretreated aromatic intermediate also contained small amounts of impurities such as benzene, xylenes, C9 aromatics, and naphthalenes. The presence of these impurities in the aromatic intermediate reduced the selectivity of benzaldehyde (Table S2 in SM).

      FIG. 5 shows influence of reaction conditions on bio-based benzaldehyde synthesis (using preferred CoFe2O4@Biochar(HTR) catalyst). As present in FIG. 5(a), substrate conversion strengthened mildly as temperature was raised from 30 °C to 70 °C but decreased slightly upon a further increase above 70 °C. This may be attributed to thermal decomposition of H2O2 into water and oxygen at higher temperature, leading to a reduction in the formation of hydroxyl radicals [20]. As the temperature exceeded 70 °C, the selectivity toward benzaldehyde lowered significantly, while by-product selectivity (especially benzoic acid) expanded (FIG. 5(b)), inferring that high temperature is favorable for benzaldehyde’s deep oxidation to benzoic acid [20]. Thus, the maximum benzaldehyde yield (46.7%) was achieved at 70 °C. As present in FIG. 5(c), the conversion was positively correlated with reaction time. When reaction time exceeded three hours, the selectivity of benzaldehyde tended to reduce, while by-product’s selectivity of benzoic acid enhanced (FIG. 5(d)). As present in FIG. S1 (SM), the conversion improved with raising the molar ratio of reactant/H2O2. When the molar ratio of reactant/H2O2 was greater than 1:3, benzaldehyde selectivity lowered, while benzoic-acid selectivity strengthened. According to benzaldehyde yield, the optimized reaction condition was as follows: a temperature of 70 °C, a reactant/H2O2 molar ratio of 1:3, and a reaction time of 3 h.

    • FIG. S2(a) in SM presents the stability and reusability of the preferred CoFe2O4@Biochar(HTR) catalyst in benzaldehyde synthesis process. After eight cycles, reactant’s conversion and benzaldehyde’s yield only slightly abated, inferring that the CoFe2O4@Biochar(HTR) catalyst possessed a competent reusability for benzaldehyde synthesis process. To understand slow deactivation of catalyst, we analyzed characteristic changes of the preferred CoFe2O4@Biochar(HTR) catalyst after the reaction. As present in FIG. S2(b) (SM), XRD pattern derived from the used catalyst is almost identical to fresh catalyst, inferring that catalyst’s structure did not undergo significant change during benzaldehyde synthesis process. Based on XPS characterization (FIG. S3 in SM), the fresh CoFe2O4@Biochar(HTR) catalyst shows a higher Fe2+/Fe3+ ratio (0.78) than the used catalyst (0.72). This indicated that Fe2+ species in fresh catalyst were partially oxidized to Fe3+ during the benzaldehyde synthesis.

      As present in FIG. S4(a) (SM), the leaching amount of metal ions in the synthesis process of benzaldehyde was measured by ICP-MS method [17]. CoFe2O4@Biochar (HTR) catalyst shows lower leaching rate of Co ions (5.3 mg·L−1h−1) than Co3O4 catalyst (11.9 mg·L−1h−1). The leaching rate of iron ion for CoFe2O4@Biochar(HTR) catalyst is 0.9 mg·L−1h−1, lower than Fe2O3 catalyst (3.6 mg·L−1h−1). This means that magnetic CoFe2O4@Biochar(HTR) catalyst is more stable compared to single metal oxide catalysts. As can be seen from FIG. S4(b) (SM), the used CoFe2O4(HTR) catalyst shows weaker EPR signal compared to fresh catalyst. This further confirmed that compared to fresh catalysts, the used CoFe2O4(HTR) catalyst had lower catalytic activity in forming hydroxyl radicals. Based on the above characterizations, the deactivation of CoFe2O4@Biochar(HTR) catalyst may be mainly attributed to the changes in valence state and the leaching of metal ions during catalytic reaction process [17].

    • To identify the active radicals in the benzaldehyde synthesis process, the EPR analysis was performed using DMPO (dimethyl-1-oxo-N-oxide) as a radical capture agent (FIG. S5 in SM). Without a catalyst, an EPR signal was very weak, confirming that it was difficult to generate hydroxyl radicals through self-decomposition of H2O2 [17]. For all Co-Fe composite metal oxide catalysts, EPR signal was observed (intensity ratio of 1:2:2:1), indicating that these catalysts can activate H2O2 to produce ·OH radicals [26]. CoFe2O4@Biochar(HTR) catalyst shows stronger EPR signal than CoFe2O4(HTR) catalyst. Based on XPS characterization (FIG. 2), the addition of biochar carrier into the CoFe2O4 (HTR) catalyst increased the ratio of Fe2+/Fe3+ in the catalyst. Considering that Fe2+ species have higher activity than Fe3+ species [17], CoFe2O4@Biochar(HTR) catalyst can get more hydroxyl radicals by catalytic decomposition of H2O2. Based on previous study [17], Fe2+ species in Co-Fe composite catalyst can initiate the decomposition of H2O2 to generate ·OH and Fe3+ (Eq.(1)), and subsequently, Fe3+ species can react with H2O2 to form Fe2+ and ·O2H (Eq.(2)). Similarly, Co2+ species in the catalyst can promote the decomposition of H2O2 to generate ·OH and Co3+ (Eq.(3)) [26]. In addition, oxygen vacancy (Ov) can also act as active center to decompose H2O2 to generate ·OH (Eq.(5)) [34].

      In this work, bio-based benzaldehyde was able to produce via coupling catalytic pyrolysis of biomass with directive oxidation of toluene intermediate. Based on analysis of radical species and previous research [8, 20, 25, 26, 35], we proposed probable mechanism for catalytic synthesis of bio-based benzaldehyde (FIG. 6). As a starting step, biomass was first converted into a toluene intermediate through catalytic pyrolysis process with a 5%Zn@HZSM-5 composite catalyst [20]. According to our previous research [20], the main active centers of the 5%Zn@HZSM-5 composite catalyst include Brønsted acid sites, Lewis acid sites, and Zn ions. The main reaction pathways in catalytic pyrolysis process of biomass mainly included biomass pyrolysis, catalytic deoxygenation, olefin aromatization and aromatic polymerization [20, 25].

      Subsequently, the toluene intermediate can be selectively converted into bio-based benzaldehyde over the CoFe2O4@Biochar(HTR) catalyst. When adopting a metal oxide catalyst and H2O2 oxidant, catalytic oxidation of toluene into benzaldehyde generally follows a free radical reaction mechanism (FIG. 6) [8, 35]. Firstly, the CoFe2O4@Biochar(HTR) catalyst can activate H2O2 to produce ·OH radicals (FIG. S5). In subsequent side chain oxidation process, ·OH radicals abstract a hydrogen atom from methyl group of toluene, generating a benzyl radical (PhCH2·) [8, 35]. The PhCH2· species is further oxidized via ·OH radicals to get benzyl alcohol, benzaldehyde as well as benzoic-acid (FIG. 6) [8, 35]. Besides, the cresol by-product was also observed (FIG. 5), which was attributed to toluene hydroxylation [8, 35]. For the hydroxylation of toluene, hydroxyl radical is embedded to C(sp2)−H bond in aromatic ring to generate CH3PhOH2· intermediate, which is then deprotonated into cresol (FIG. 6) [8, 35].

    IV.   CONCLUSION
    • In this study, we developed a new approach for synthesizing bio-based benzaldehyde. This controllable transformation is based on uniting catalytic pyrolysis of lignocellulose and toluene oxidation. This work developed a highly active catalyst (CoFe2O4@Biochar (HTR)) and proved its suitability for the selective synthesis of benzaldehyde. The magnetic CoFe2O4@ Biochar(HTR) catalyst exhibited good benzaldehyde selectivity (77.1%) and benzaldehyde yield (46.7%). The catalyst characterization proved that the introduction of biochar support into the Co-Fe composite metal oxide catalyst reduced particle aggregation and increased the Fe2+/Fe3+ ratio, which was beneficial for the formation of ·OH radicals and the synthesis of benzaldehyde. The probable reaction mechanism for bio-based benzaldehyde synthesis was proposed, based on catalyst characterization and hydroxyl radical analysis.

      Supplementary materials: Compositions of crude aromatic intermediate and pretreated aromatic intermediate are shown in Table S1. Catalytic performance of different catalysts in bio-benzaldehyde synthesis is given in Table S2. Effect of molar ratio of reactant:H2O2 on bio-benzaldehyde synthesis is given in FIG. S1. Stability of catalysts is given in FIG. S2(a). XRD patterns of fresh/used CoFe2O4@Biochar(HTR) catalyst are given in FIG. S2(b). Fe 2p XPS spectra of fresh/used CoFe2O4@Biochar(HTR) catalyst are given in FIG. S3(a). Co 2p XPS spectra of fresh/used CoFe2O4@ Biochar(HTR) catalyst are given in FIG. S3(b). O 1s XPS spectra of fresh/used CoFe2O4@Biochar(HTR) catalyst are given in FIG. S3(c). Iron and cobalt ion leaching in catalytic reaction process are given in FIG. S4(a). EPR spectra of ·OH-DMPO radicals using fresh and used CoFe2O4@Biochar(HTR)catalysts are shown in FIG. S4(b). EPR spectra of ·OH-DMPO radicals obtained from different catalytic reaction systems are given in FIG. S5.

    Figure (6)  Reference (35)