Metal/semiconductor heterointerfaces are among the most consequential junctions in modern technology, governing key processes in electronic components, opto-electronic devices, photochemistry, and heterogeneous catalysis [1−8]. These heterointerfaces often exhibit enhanced functionalities that cannot be achieved by the isolated constituents, because interfacial coupling reshapes charge separation, reaction energetics, and light–matter interactions. At the nanoscale, semiconductor substrates can host metal clusters with dimensions of only a few nanometers [5, 9−11]. In this regime, localized surface plasmon resonances can strongly concentrate optical fields, thereby enhancing optical absorption, exciton generation, and interfacial charge transfer [12−15]. Conversely, metal substrates can serve as conductive supports for oxide films or clusters [8, 16, 17], where electronic coupling across the buried interface profoundly modifies the oxide electronic structure [18]. A particularly important consequence is the penetration of metal wavefunctions into the adjacent oxide, producing interface-derived states within the band gap, commonly referred to as metal-induced gap states (MIGSs) [19]. MIGSs provide a high density of interfacial electronic states that frequently leads to Fermi-level (EF) pinning, thereby dictating band alignment, barrier heights, and charge-transfer driving forces [9, 11, 20−23]. Beyond pinning, MIGSs may act as preferential sites for charge accumulation and interfacial hybridization, suggesting that they could serve as optically addressable “gateways” for optical excitations across metal/oxide interfaces [24].
Optical response in semiconducting oxides is typically dominated by valence band maximum (VBM) to conduction-band minimum (CBM) transitions, and band-gap engineering remains a central strategy to tailor absorption and reactivity [25−28]. Conventional approaches rely on introducing defects, heteroatom impurities, or dopants that reshape band edges and create gap states. Classic examples include Cr/N doping in TiO2 to extend absorption from the ultraviolet into the visible [29−31], and oxygen vacancies or hydroxyl-related defects that generate Ti 3d-derived gap states [32−37], which can enhance electrical conductivity and catalytic activity. For optical response, gap state can open sub-gap excitation, while it also behaves as a recombination center that may quench interfacial charge separation [38]. Notably, defect-induced gap states on TiO2(110) have been shown to open resonant optical excitation pathways to the conduction band, partially bypassing direct VBM–to–CBM excitation [35, 36, 39, 40]. In contrast to the defect-induced gap states, MIGS originates intrinsically from interfacial hybridization and therefore carry direct relevance to charge transfer across the junction. Despite their recognized importance in determining electronic alignment and carrier injection, how MIGSs participate in optical excitation remains insufficiently understood. A key question is whether MIGS acts as an optically active state that enable resonant population of unoccupied states, or merely provides ultrafast decay channel that quench interfacial charge separation.
Here, taking the well-defined junction consisting of monolayer (ML) Fe3O4 film grown on single-crystal Ag(100), we detect the occupied MIGS and directly trace its involvement in resonant excitation pathways into high-lying unoccupied manifolds by combining scanning tunneling microscopy/spectroscopy (STM/STS) [41, 42], angle-resolved photoemission spectroscopy (ARPES) [43, 44], and femtosecond two-photon and three-photon photoemission (2PP/3PP) spectroscopy [45, 46]. An occupied MIGS at 0.5 eV below EF is identified by STM in real-space and ARPES in energy-momentum space. By tuning the femtosecond pulse photon energy in the UV-visible range (
$\hbar$ ω = 5.08 eV to 1.88 eV), we reveal that optical excitation is not limited to hot-electron population of CBM. Instead, the MIGS serves as a dominant source that promotes population of high-lying unoccupied states above the CBM. Specifically, UV pulses primarily access these states through one-photon excitation steps, whereas visible pulses drive two-photon resonant excitation into high-lying CBs and IP states near vacuum level (Evac), establishing multiple excitation channels for interfacial charge transfer from Ag(100) into Fe3O4. These findings identify MIGS as an intrinsic, interface-enabled “band-gap-engineering” lever that can steer optical excitation pathways without introducing bulk defects or dopants, offering a general strategy to tailor photoinduced charge separation and carrier injection in metal/oxide heterointerfaces. -
The single crystal Ag(100) (surface preparation laboratory) surface was cleaned by repeated Ar+ ion sputtering at 1000 eV and annealing in ultrahigh vacuum (UHV, <2×10−10 mbar) at 700 K for multiple cycles. Iron atoms were deposited to Ag(100) surface held at ~500 K using an electron beam evaporator (FOCUS GmbH) under the background oxygen pressure of 5×10−6 mbar. Subsequently, the sample was annealed for 10 min in the same oxygen pressure, followed by an additional 5-min annealing under ultra-high vacuum conditions to form pure iron oxide islands.
-
The STM measurements were carried out at the liquid helium temperature (~5 K) in a Unisoku USM1400-LT Scanning Probe Microscope equipped with a Nanonis controller, under ultrahigh vacuum (<2×10−10 mbar). An electrochemically etched Ag tip was employed for STM imaging, and the bias was applied to sample with respect to the tip. The dI/dV experiments were performed through a lock-in amplifier with a modulation of 10 mV at 937 Hz.
The ARPES and X-ray photoelectron spectroscopy (XPS) measurements were excited by a resonance helium discharge lamp (He I, 21.2 eV and He II, 40.8 eV) and Al Kα radiation (1486.6 eV), respectively. A hemispherical energy analyzer (VG Scienta, DA30L) was used to record the 2D E(k) maps of the kinetic energy and momentum of the photoelectrons from the sample for ARPES measurements. The energy resolution is ~30 meV and the angular resolution is better than 0.1°. All measurements were conducted in analysis chamber with a base pressure of 5×10−11 mbar.
Wavelength-tunable excitation pulse trains were generated by a self-built femtosecond noncollinear optical parametric amplifier (NOPA), which was pumped by a 1030 nm femtosecond laser (Light conversion, Pharos-20W) operating at a 500 kHz repetition rate. The NOPA was tuned between 490−870 nm (
$\hbar $ ω=1.43−2.53 eV) with an average output power of 60 mW to 80 mW. Multiple reflections from a matched pair of negative dispersion mirrors compressed the pulses to near-transform limited duration of ~30 fs at the sample surface. The pulses were frequency doubled to 247−435 nm ($\hbar $ ω=2.85−5.02 eV) using a BBO crystal and compressed to ~20−30 fs through multiple reflections from a matched pair of negative dispersion mirrors.The 2PP/3PP measurements were carried out at room temperature in a UHV chamber with a base pressure of 1.5×10−10 mbar. The 2PP/3PP spectra were acquired using a hemispherical electron energy analyzer (Specs, Phoibos 150, ±15° acceptance angle). A 2D DLD delay-line detector (Surface Concept) recorded the final state energy (Efinal) values in single photoelectrons counting acquisition mode. A bias of 3 V was applied between the sample and the analyzer to collect low-energy photoelectrons.
-
Iron oxides have been extensively grown on single-crystal metal surfaces [47−49], providing well-defined model systems for studying the optical response. Typically, FeOx films are prepared under ultrahigh vacuum by depositing Fe atoms followed by post-annealing in an O2 atmosphere, which offers fine control over film composition and thickness. However, such straightforward oxidation of Fe atoms leads to three-dimensional islanding rather than uniform, layer-by-layer growth [50, 51]. The resulting stoichiometry and crystallographic orientation are highly sensitive to the choice of substrate, oxidation protocol, annealing conditions. Recent studies have nonetheless demonstrated that nanometer-thick FeOx films with tunable stoichiometry can be reliably stabilized on Ag(100) by carefully optimizing growth parameters [52−55]. Building on these advances, we achieved a pure Fe3O4 monolayer on Ag(100) by precisely controlling the oxygen partial pressure and deposition temperature.
FIG. 1(a) shows a representative STM image of monolayer Fe3O4 islands grown on Ag(100) with a coverage of ~0.4 monolayer. The iron-oxide film forms predominantly hexagonal islands, with a fraction nucleating and extending along substrate step edges. FIG. 1(b) is a magnified image revealing an atomically resolved hexagonal lattice that is clearly incommensurate with the square symmetry of the Ag(100) surface. The average lattice constant is approximately 0.319 nm, ~10% larger than the Ag(100) surface lattice constant (0.289 nm). This lattice mismatch gives rise to a larger periodic moiré superstructure. As seen in FIG. 1(a), the moiré corrugations are oriented along the two high-symmetry directions of the Ag(100) substrate. FIG. 1(c) displays the line profile along the white dashed line in FIG. 1(a), corresponding to the white dashed line, yielding a moiré periodicity of 3.76 nm. An apparent island height of ~0.21 nm is obtained, which is consistent with the height of a monolayer. Based on the measured Fe–Fe spacing of 0.319 nm (FIG. 1(d)), we assign the islands to monolayer magnetite (Fe3O4) [56, 57].
To further verify the Fe3O4 stoichiometry, we perform X-ray photoelectron spectroscopy measurements. The O 1s XPS spectrum exhibits a sharp peak centered at ~530.1 eV, consistent with lattice oxygen in iron oxides (FIG. 1(e)). The Fe 2p region is more challenging to interpret because it overlaps with the Ag 3s emission from the substrate. Nevertheless, the spectrum in FIG. 1(f) clearly shows the Fe 2p3/2 and Fe 2p1/2 peaks at 711.1 eV and 723.5 eV, respectively. The broad line shapes indicate that the Fe 2p signal cannot be described by a single chemical state. The presence of two broad features suggests that the components likely do not originate from one single state. Peak deconvolution further reveals a strong contribution from the Ag substrate around 719 eV [58], and indicates that both the Fe 2p3/2 and Fe 2p1/2 envelopes contain components associated with two iron valence states, with the Fe2+ component appearing at slightly lower binding energy than Fe3+. In addition, characteristic shake-up satellite features are observed on the higher-binding-energy side of both spin–orbit components. Together, these signatures demonstrate a mixed-valence Fe2+/Fe3+ character, strongly supporting assignment of the islands to magnetite [51, 57].
-
We measured the local electronic states by STS spectra across the terraces of Ag(100) and Fe3O4 islands (FIG. 2(a)). The normalized dI/dV spectra are presented as a heat map in FIG. 2(b), with the lateral distance indicating the positions marked by the black arrow in FIG. 2(a). The lower and upper panels in FIG. 2(b) are measured by constant height mode dI/dV and constant current mode dZ/dV, respectively, to show the electronic states near EF and high energies near Evac. In the upper panel, the application of a higher bias voltage between the STM tip and the sample causes the resonant tunneling of electrons through the potential barrier as standing waves, generating a series of sharp current peaks in the dZ/dV spectrum [59, 60]. The peak located at ~4.7 V for bare Ag(100) in FIG. 2(b) corresponds to the n=1 field emission resonance (FER). This peak shifts to ~5.2 V on the iron oxide island, indicating that the local work function of the iron oxide is approximately 0.5 eV higher than that of Ag(100) substrate [61, 62]. Higher order FER peaks are shown in FIG. S1 (in Supplementary materials, SM). In addition, two unoccupied conduction bands (CB1 and CB2) are observed on iron oxide.
The lower panel of FIG. 2(b) clearly shows the VBM at about −2.0 eV and CBM at ~0.3 eV for iron oxide, giving a bandgap of ~2.3 eV. The measured bandgap is comparable to the ~2–3 eV gaps reported for nanoscale Fe3O4 particles and ultrathin films [63−65], yet it differs markedly from the half-metallic behavior of bulk Fe3O4. This contrast arises because bulk Fe3O4 adopts an inverse-spinel structure, in which mixed-valence Fe2+/Fe3+ ions on the octahedral B sublattice support electron hopping, yielding a finite density of states at the Fermi level and thus metallic conductivity. In addition, a distinct MIGS appears at Eb=−0.5 eV with an energy broadening of ±0.2 eV. It is noteworthy that the MIGS uniformly distributes across the entire defect-free iron oxide terrace, in contrast to MIGS induced by defect site or edge site on other oxide surfaces [32, 33]. We therefore attribute the MIGS to an intrinsic property of the Fe3O4/Ag(100) interface. We further examine the MIGS by ARPES measurements. A uniform, defect-free iron oxide film was successfully grown on Ag(100) with a coverage close to 1 ML (FIG. 2(c)). The 2D E(k) maps of bare Ag(100) and 1 ML Fe3O4/Ag(100) are compared in FIG. 2(d). After being covered by the iron oxide film, the sharp sp band of Ag(100) becomes faint, and notably, the VBM can be observed at −2.0 eV and a weak MIGS arises just below the EF. The corresponding second derivative map and the energy distribution curve (EDC) in the range of 0 to −2.5 eV amplify the characteristics of the VBM and MIGS in FIG. 2(e), in good agreement with those in the STS spectra (lower panel of FIG. 2(b)).
-
We investigated the excitation pathways at the Fe3O4/Ag(100) interface by performing ultrafast angle-resolved 2PP spectroscopy. Femtosecond UV pulses with a energy range of
$\hbar $ ω=2.85 eV to 5.02 eV can cause a two-photon pump-probe process, where the first photon pumps an electron from the occupied bands to an intermediate state, and the second photon probes the electron above Evac into photoemission continuum. The photoemitted electrons are recorded as a 2D Efinal(k) map, indicating the final state energy versus k||. FIG. 3(a)−(d) shows four representative 2PP Efinal(k) maps obtained at the Fe3O4/Ag(100) interface with ~1 ML coverage excited by different$\hbar $ ω. All the four Efinal(k) maps indicate the lowest Efinal=5.1 eV, corresponding to the surface work function. The black horizontal lines indicate the highest detectable Efinal, which is excited by 2$\hbar $ ω from EF. 2PP Efinal(k) in FIG. 3(a) shows the main features of “MIGS” with a flat band character and the dispersive “CB1”, as indicated by the white and red dashed lines, respectively. The assignment is further validated by determining their binding energy in FIG. 3(b)−(d). It is noteworthy that in FIG. 3(a), the “MIGS” feature indicates a direct two-photon excitation by 2$\hbar $ ω=6.36 eV from its occupied initial state, while the “CB1” feature indicates an indirect population from the virtual intermediate state followed by the one-photon photoemission (sketched in FIG. S2 in SM). These two-photon and one-photon excitation processes for “MIGS” and “CB1”, respectively, make their final state energy changes in different steps of 2Δ$\hbar $ ω and 1Δ$\hbar $ ω when tuning the photon energies in FIG. 3(a)−(d). For instance, by comparing FIG. 3(a, b) it is shown that the Δ$\hbar $ ω=0.58 eV causes ~0.55 eV upshift of “CB1” and ~1.1 eV upshift of “MIGS” of their Efinal. In addition, FIG. 3(b) shows an intense, featureless hot electron distribution at lower Efinal, which could be attributed to bandgap excitation producing thermalized electrons to CBM. Increasing the excitation$\hbar $ ω to 3.94 eV (FIG. 3(c) and FIG. S3 in SM), the “CB2” becomes visible in the 2PP Efinal(k) map. It can be learnt from the binding energy difference between MIGS and CB2 in FIG. 2(b), the excitation by$\hbar $ ω=3.94 eV from MIGS can populate the “CB2”, and thus makes it visible in the 2PP Efinal(k) map. Further increasing excitation$\hbar $ ω to 4.81 eV (FIG. 3(d)) makes two additional dispersive bands visible, which are assigned to the image potential states of Ag(100) and Fe3O4 film, respectively.From the above spectral analysis, it is shown that the occupied “MIGS” just below EF behaves as an effective electron source initializing optical excitation. The UV excitation from “MIGS” can promote the electrons by 1
$\hbar $ ω to high energies, which can populate and reside in the unoccupied “CB1”, “CB2”, as well as the IP states. In contrast, excitation from the VBM lying deep below −2.0 eV fail to provide enough energy to populate the higher-lying state, but generates a hot electron distribution in CBM. To further rationalize these excitation pathways, a series of line profiles extracted from k|| = 0 Å−1 are plotted as a function of excitation$\hbar $ ω in the 2D color form (FIG. 3(e)). The “MIGS” appears with its energy shifting in the same step of 2$\hbar $ ω.Sequentially, the branches of CB1, CB2, IPAg, and
$ {\text{IP}}_{{{\text{Fe}}_{3}}{{\mathrm{O}}_{4}}} $ appear at distinct$\hbar $ ω. In addition, the hot electrons distribute in the low Efinal energy range. From these line profiles, the Efinal of each state can be extracted and plotted against$\hbar $ ω (FIG. 3(f)). The linear fitting gives the approximate slopes, s≈2 for “MIGS”, and s≈1 for “CB1”, “CB2”, “IPAg”, and “$ {\text{IP}}_{{{\text{Fe}}_{3}}{{\mathrm{O}}_{4}}} $ ”, demonstrating their nature as two-photon excitation from an initial occupied state, and one-photon excitation from an intermediate unoccupied state, respectively. From the linear fitting, the binding energy of each state can be converted using Efinal–s·$\hbar $ ω (FIG. 3(g)). The vertical arrows in FIG. 3(g) indicate the minimum$\hbar $ ω that the MIGS electrons can be excited to populate each high-lying unoccupied state. In contrast, the excitation from the deeper VBM is less efficient and requires high$\hbar $ ω. When$\hbar $ ω is above 4.5 eV, the CBM→CB1 transition can be achieved (the blue arrow in FIG. 3(g)). In fact, from the normalized intensities, the VBM→CB1 transition is less efficient as compared with the MIGS→CB1 transition. -
We next tuned the excitation with photon energy in the visible range of
$\hbar $ ω=1.88−2.53 eV, where three photons are required to overcome the surface work function to induce photoemission. Typical 3PP Efinal(k) maps excited by$\hbar $ ω=2.0 eV on bare Ag(100) and Fe3O4/Ag(100) are compared in FIG. 4(a, b). At the bare Ag(100) surface, the Efinal(k) map shows a surface work function of ~4.6 eV and a dominant feature of IPAg at Efinal of ~5.9 eV. The IPAg is a common feature converging to ~0.7 eV below the Evac. At the Fe3O4/Ag(100) interface, the Efinal(k) map shows that the surface work function increases to ~5.1 eV, while the IPAg is preserved at Efinal of ~5.9 eV, and meanwhile, two new bands labeled as “$ {\text{IP}}_{{{\text{Fe}}_{3}}{{\mathrm{O}}_{4}}} $ ”and “CB2” appear at Efinal of ~6.5 eV and ~5.4 eV, respectively. By tuning$\hbar $ ω from 2.0 eV (FIG. 4(b)) to 2.07 eV (FIG. 4(c)) and 2.34 eV (FIG. 4(d)), it can be seen that the state energies upshift in the step of 1Δ$\hbar $ ω, indicating they are pumped by two-photon excitation and probed by one additional photon in the overall three-photon process.Notably, the relative intensities of “IPAg” and “
$ {\text{IP}}_{{{\text{Fe}}_{3}}{{\mathrm{O}}_{4}}} $ ” are reversed in FIG. 4(c, d), indicating distinct excitation processes that populate the “IPAg” and “$ {\text{IP}}_{{{\text{Fe}}_{3}}{{\mathrm{O}}_{4}}} $ ” when tuning the$\hbar $ ω (wavelength). To verify this, a series of line profiles extracted from the 3PP spectra are plotted in the 3D waterfall plot. By normalizing the spectral intensities at the work function edge [23, 45, 46, 66], the resonant intensifications of “IPAg” and “$ \text{IP}_{\text{Fe}_3\text{O}_4} $ ” appear at specific wavelengths of 600 nm (2.07 eV) and 530 nm (2.34 eV), respectively. To figure out the resonant excitation process, we plotted the relationship between the Efinal energies of “IPAg” and “$ {\text{IP}}_{{{\text{Fe}}_{3}}{{\mathrm{O}}_{4}}} $ ” versus$\hbar $ ω in FIG. 4(f). Based on linear fitting, the binding energies of 3.82 eV and 4.46 eV are determined for “IPAg” and “$ {\text{IP}}_{{{\text{Fe}}_{3}}{{\mathrm{O}}_{4}}} $ ”, in consistence with the values obtained in FIG. 3(g). Further plotting the normalized intensities of “IPAg” and “$ {\text{IP}}_{{{\text{Fe}}_{3}}{{\mathrm{O}}_{4}}} $ ” as a function of$\hbar $ ω locates the resonant conditions at$\hbar $ ω=2.07 and 2.34 eV, respectively. From the binding energies and the resonant$\hbar $ ω, we can deduce that an initial occupied state at ~0.3 eV below EF by Efinal−2$\hbar $ ω. This position points to the upper edge of the MIGS at −0.5±0.2 eV. We thus attribute the two-photon resonances from MIGS which are responsible for the optical transitions under visible excitation. -
Optical excitation in semiconductors typically generates hot electrons that rapidly relax toward the CBM through electron–electron and electron–phonon scattering. In contrast, the generation and stabilization of high-energy electrons in high-lying unoccupied CBs above the CBM, as well as in IP states near the Evac, are particularly intriguing for photochemistry and optoelectronic applications, as these energetic carriers can deliver substantially higher excess energies to drive charge transfer and chemical reactions. Recent studies have demonstrated that populating high-lying electronic states can lead to fundamentally different excitation pathways and functionalities. For example, population of the high-lying interlayer band in graphite near the Evac enables intense thermionic emission [67], while excitation into high-lying conduction bands in layered materials can give rise to high-lying excitons with distinct optical selection rules [46, 68]. However, in typical oxide semiconductors such as Fe3O4 and TiO2, the VBM lies deep ( > 2 eV) below EF. As a result, UV and visible light excitation can rarely access high-lying unoccupied states, limiting optical excitations to band-edge transitions and restricting the generation of energetic charge carriers. Our results demonstrate that the presence of MIGS at the Fe3O4/Ag(100) interface fundamentally alters this limitation. The MIGSs introduce electronic states within the band gap that serve as efficient source states for optical excitation, thereby opening new excitation channels that are inaccessible in isolated oxide systems.
Importantly, the electronic states involved in these processes are spatially distinct: the MIGS are intrinsic to the Fe3O4/Ag(100) interface, the conduction bands are a property of the monolayer Fe3O4 film, and the IPs possess density of states located above the surface. Consequently, optical excitations of MIGS→CBs and MIGS→IP naturally involve charge transfer across the metal/oxide interface, leading to pronounced spatial separation of electrons and holes. This interfacial charge separation can significantly prolong carrier lifetimes, in sharp contrast to isolated oxides, where gap states typically act as recombination centers that quench photoexcited carriers. The interfacial nature of the MIGSs therefore converts gap states from detrimental recombination sites into functional gateways for efficient charge separation and energy conversion.
In summary, by taking Fe3O4/Ag(100) as a prototypical metal/oxide interface, we identify and realize multiple optical excitation pathways from metal-induced gap states to high-lying unoccupied electronic states. These processes establish efficient and spatially separated charge transfer channels across the interface, enabling the generation of long-lived energetic electrons. The combination of STM/STS, ARPES, and ultrafast 2PP/3PP spectroscopy provides a multidimensional perspective for resolving the excitation mechanisms and electronic structure underlying these phenomena. Our findings highlight the critical role of interfacial electronic states in governing high-energy optical excitations and suggest a general strategy for engineering energetic charge carriers at metal/oxide interfaces, with broad implications for photocatalysis, optoelectronics, and interfacial energy conversion.
Multiple Optical Excitation Pathways at Fe3O4/Ag(100) Interface Enabled by Metal-Induced Gap State
- Received Date: 28/01/2026
- Available Online: 27/10/2026
-
Key words:
- Metal-oxide heterojunction /
- Scanning tunneling microscopy /
- Angle-resolved photoemission spectroscopy /
- Ultrafast spectroscopy /
- Photochemistry
Abstract: Optical excitation in bulk oxide semiconductors predominantly proceeds via band-edge transitions, generating hot carriers near the conduction-band minimum (CBM). However, populating high-lying unoccupied states above the CBM is often less efficient because of energy-momentum constraints and weak transition dipole moments. Here, using a prototypical metal/oxide junction consisting of monolayer Fe3O4 on Ag(100), we show that a metal-induced gap state (MIGS) created by strong interfacial hybridization serves as the dominant electronic reservoir for accessing high-lying unoccupied conduction bands (CBs) and image potential (IP) states near vacuum level. Beyond hot-electron population of the CBM, the MIGS provides efficient pathways for MIGS→CB and MIGS→IP transitions, whereas valence-band contributions are secondary. These excitations establish pronounced spatial charge separation across the Fe3O4/Ag(100) interface, in contrast to isolated oxides where gap states typically act as recombination centers. Our results highlight interfacial electronic-structure engineering as an effective strategy to generate energetic carriers for photocatalysis and optoelectronic applications.
首页
登录
注册


DownLoad: