2024 Volume 33 Issue 6
Article Contents

Wan-Li Zhu, Wei-Li Zhen, Rui Niu, Ke-Ke Jiao, Zhi-Lai Yue, Hui-Jie Hu, Fei Xue, Chang-Jin Zhang. Linear dichroism transition and polarization-sensitive photodetector of quasi-one-dimensional palladium bromide[J]. Chinese Physics B, 2024, 33(6): 068101. doi: 10.1088/1674-1056/ad36ba
Citation: Wan-Li Zhu, Wei-Li Zhen, Rui Niu, Ke-Ke Jiao, Zhi-Lai Yue, Hui-Jie Hu, Fei Xue, Chang-Jin Zhang. Linear dichroism transition and polarization-sensitive photodetector of quasi-one-dimensional palladium bromide[J]. Chinese Physics B, 2024, 33(6): 068101. doi: 10.1088/1674-1056/ad36ba

Linear dichroism transition and polarization-sensitive photodetector of quasi-one-dimensional palladium bromide

通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(5)

Article Metrics

Article views(179) PDF downloads(0) Cited by(0)

Access History

Linear dichroism transition and polarization-sensitive photodetector of quasi-one-dimensional palladium bromide

Abstract: Perpendicular optical reversal of the linear dichroism transition has promising applications in polarization-sensitive optoelectronic devices. We perform a systematical study on the in-plane optical anisotropy of quasi-one-dimensional PdBr2 by using combined measurements of the angle-resolved polarized Raman spectroscopy (ARPRS) and anisotropic optical absorption spectrum. The analyses of ARPRS data validate the anisotropic Raman properties of the PdBr2 flake. And anisotropic optical absorption spectrum of PdBr2 nanoflake demonstrates distinct optical linear dichroism reversal. Photodetector constructed by PdBr2 nanowire exhibits high responsivity of 747 A⋅W−1 and specific detectivity of 5.8 × 1012 Jones. And the photodetector demonstrates prominent polarization-sensitive photoresponsivity under 405-nm light irradiation with large photocurrent anisotropy ratio of 1.56, which is superior to those of most of previously reported quasi-one-dimensional counterparts. Our study offers fundamental insights into the strong optical anisotropy exhibited by PdBr2, establishing it as a promising candidate for miniaturization and integration trends of polarization-related applications.

1.   Introduction
  • Optical information detection has always been a primary way for humans to perceive the external world.[1] Light is an electromagnetic wave that consists of key elements information like intensity, wavelength, phase, and polarization.[2] Polarized light detection technology plays an important role in the fields of optical fiber communication, environmental monitoring, and remote imaging.[3–5] In contrast to traditional photodetectors, polarized photodetectors show the ability to extract light polarization to provide more and clearer information about the imaged objects (e.g., surface roughness, geometry or orientation).[6–8] The development of polarization-sensitive devices is of crucial importance for meeting with the requirements of miniaturization, compactness, and high integration.[9,10]

    The versatility and engineerability of low-dimensional materials enable them to play superior roles in development of polarization-sensitive devices.[4,11–13] For instance, by combining different types of low-dimensional materials, the spectral response range of opto-devices can be significantly broadened.[14–18] And low-dimensional materials can affect their physical properties through surface defect states or local fields,[19–21] which provide opportunities to optimize polarized light detectors. Nanowire-based polarized photodetectors have gained significant recognition for their compact device size, exceptional conversion efficiency, adjustable light absorption coefficient, and wide spectral range.[22–29] This is particularly important in the context of industrial market demand for device integration and miniaturization. Searching for new polarization-sensitive low-dimensional materials has long been a research frontier.

    Low-dimensional transition metal halides (TMHs) have received much attention due to their diverse optoelectronic properties,[30,31] topological magneton and electromagnetic properties,[32–34] and broad applications in spintronics.[35,36] Palladium bromide (PdBr2), a recently reported TMH with quasi-one-dimensional structure, has become the center of research due to its ultrahigh current carrying capacity,[37] bipolar magnetic semiconducting properties,[38] and ultra-sensitive photoresponse for photodetectors and field-effect transistors.[39] Here, we present experiments systematically revealing in-plane optical anisotropy of PdBr2, including the angle resolved polarized Raman spectroscopy (ARPRS), and anisotropic optical absorption spectrum. The ARPRS data validate the anisotropic phonon vibration properties and the crystal structure orientation of the PdBr2 flake. And the angle-resolved absorption spectrum of the PdBr2 nanoflake reveals the in-plane anisotropic optical properties. A peculiar occurrence of polarization reversal is detected at 397 nm, exhibiting perpendicular optical linear dichroism (LD) reversal. High-performance polarization photodetector constructed by PdBr2 nanowire has been achieved, which exhibits responsivity of 747 A⋅W−1, specific detectivity of 5.8 × 1012 Jones and strong polarization-sensitive photoresponsivity (photocurrent anisotropic ratio of 1.56) under the 405-nm light irradiation, respectively. Our study offers essential insights into the optical anisotropy exhibited by PdBr2. The remarkable anisotropic characteristics and semiconductor nature make PdBr2 a captivating contender for applications involving polarization imaging, which facilitates the exploration of downsizing trends in polarization-resolved detectors and expands the potential applications of quasi-one-dimensional materials towards the advancement of optoelectronic devices with low-dimensional polarization sensitivity in the future.

2.   Experiment
  • Needle-like single crystals of PdBr2 were synthesized through the physical vapor transport (PVT) method. An evacuated quartz tube was utilized to contain 200 mg of PdBr2 powder (with purity of 99.99%, purchased from Alfa Aesar) under vacuum condition (< 10−4 Torr, 1 Torr = 1.33322×102 Pa). The tube was positioned within a horizontal double-zone tube furnace, with the source and growth zones being heated to 973 K and 673 K, respectively. The tube was kept at these temperatures for 7 days and then cooled down naturally.

    A Rigaku-TTR3 x-ray diffractometer with Cu Kα radiation was used for single crystal x-ray diffraction measurements. The angle-resolved polarized Raman spectroscopy measurements were conducted using a Horiba Jobin Yvon confocal Raman spectrometer (LabRam800HR). The polarized absorption spectra of the nanoflake sample was collected using a micro-zone absorption spectrometer (MStarter ABS, Metatest Co. Ltd.). The two-terminal devices were fabricated by transferring the PdBr2 channel material to the pre-prepared electrodes using polydimethylsiloxane (PDMS) as the carrier. Figure S1 shows the optical microscope image of the mechanically exfoliated PdBr2 nanoflakes and nanowires on a PDMS substrate. The ease of stripping PdBr2 into nanowires could be due to its quasi-one-dimensional chain structure. The electrical and optoelectronic measurements were carried out using a home-made multi measurement system equipped with a Keithley 2636B source meter and a four-probe station. The 405-nm polarized laser was obtained through a Glan Taylor prism and a half wave plate. The power of the incident laser was calibrated by a power meter (PM100D, Thorlabs), and the laser spot diameter of 5 mm was sufficient to uniformly cover the entire device channel area.

3.   Results and discussion
  • Figure 1(a) displays the schematic structure of PdBr2 with different view directions. PdBr2 belongs to the monoclinic crystal structure with the space group P21/c (No. 14, a = 6.59 Å, b = 3.96 Å, c = 25.22 Å, and α, γ = 90°, β = 92.6°). In this structure, weak van der Waals interactions bundle together one-dimensional (1D) chains that solely possess covalent bonds along chain direction. Single crystal x-ray diffraction patterns of the obtained grown samples showed sharp diffraction peaks (Fig. 1(b)) that matched well with the standard PDF card (PDF#76-1621) of PdBr2 crystal, indicating the high crystallinity. The length of the obtained PdBr2 single crystals could be longer than 1 cm, as shown in the inset of Fig. 1(b). To comprehensively investigate the electronic properties of monoclinic PdBr2, we calculated the band structure of bulk PdBr2. The results are shown in Fig. 1(c). First-principles calculations are executed using the density functional theory (DFT) framework, employing projector augmented wave (PAW) potentials as implemented in the Vienna ab initio simulation package (VASP). For the structural relaxation part of the DFT calculations, we utilize the generalized gradient approximation (GGA) as formulated by Perdew, Burke, and Ernzerhof (PBE),[44] ensuring accurate modeling and analysis of the structural properties. The calculated bandgap is about 1.24 eV, which is close to our prior experiment results bandgap for bulk PdBr2. We also present the total and partial density of states (DOS) for PdBr2 in Fig. S2. Analysis of the projected DOS reveals that both the conduction and valence bands could be attributed to the contributions from both Pd and Br atoms. Scanning electron microscope image, energy dispersive spectroscopy elemental measurement results, and mapping plot are shown in Figs. 1(d) and 1(e), respectively. The Pd:Br atomic ratio as 33.46:66.54 of a typical flake sample indicates the stoichiometric ratio of 1:2. Figure 1(f) shows the non-polarized Raman spectrum of PdBr2. Three phonon vibration peaks at 120 cm−1–240 cm−1 (namely P1, P2, and P3) is observed, which is in good agreement with previous investigations of Raman information on bulk PdBr2 sample.[37,39]

    The symmetry of chemical bond vibration and crystal orientation can be determined using ARPRS measurement.[40,41] During the measurement, the analyzer is adjusted to align parallel and perpendicular to the laser polarization direction, respectively. The incident laser (532 nm) is polarization light and fixed horizontally, with the scattered light polarization vector aligned either parallel (XX) or perpendicular (XY) to that of the incident laser using a polarization analyzer. The ARPRS experiment is performed by incrementally rotating the sample at an interval of 30°. Figures 2(a) and 2(b) give the three-dimensional (3D) contour color mapping and two-dimensional (2D) projection of polarized Raman intensity with the rotation angles ranging from 0° to 360° in XX and XY configurations, respectively. The intensity of the Raman peaks exhibits visibly discrepancy changes depending on the polarization angle θ. The bulk PdBr2 crystal exhibits monoclinic symmetry with a C2h point group, featuring 18 phonon modes (3Ag + 6Au + 3Bg + 6Bu) at the Gamma point. Among them, six phonon modes are Raman active (3Ag + 3Bg). In our scheme, only Ag modes (P1: 163 cm−1, P2: 185 cm−1, P3: 203 cm−1) are observable in ARPRS due to the polarization selection rules of XX and XY configurations. The formula based on group theory and Raman tensors is utilized to fit the Raman intensity function with polarization angle[39,42]

    Here, a, b, and d are the tensor constants for specific Raman mode. θ is the polarization angle. Figures 2(c)–2(e) display the polar plots for the Raman peak intensity at (c) 163 cm−1, (d) 185 cm−1, and (e) 203 cm−1 as the function of polarization angles, respectively. The fitting curves in polar coordinates using Eqs. (1) and (2) agree well with the experimental data. The phonon modes, which vary with the polarization angles, provide insights into the anisotropic structure and enable one to determine the lattice orientation of PdBr2 flake. The polar plot shows that the anisotropy variation period of the P1 peak is 180°, while the period of P2 and P3 peaks is 90°. The ARPRS results reveal that the PdBr2 flakes exhibit an in-plane anisotropic structure, which motivates further exploration into their in-plane anisotropic absorbance and polarization-dependent photoresponse performances.

    We subsequently examine the absorption of polarized light by PdBr2 when exposed to a laser beam with polarization angle ranging from 0 to 180° in an interval of 45°. The results are depicted in Fig. 3(a). The angle of polarization is determined by the disparity between the orientation of light polarization vector and the a axis of the PdBr2 crystal, as shown in the inset of Fig. 3(a). It is found that the PdBr2 flake exhibits strong polarization-angle dependence of optical absorption intensities in a broad spectral range from 200 nm to 1000 nm. Interestingly, a clear occurrence of the optical reversal phenomenon can be observed. For example, the absorption gradually increases at 755 nm and gradually decreases at 350 nm within the range of 45° to 135°. The laser power remains consistent throughout our measurement, and the observed variation in absorption intensity indicates the occurrence of the LD transition of PdBr2. The LD ratio, defined as the ratio in absorption intensity parallel, and perpendicular to a-axis direction, is plotted in Fig. 3(b). By referring to the optical image in measurement, we choose the absorption intensities along 45° and 135° configurations, i.e., parallel and perpendicular to the a-axis direction, to investigate the LD of PdBr2 nanoflakes. Comparisons of two kinds of dichroism ratio modes (red line, α-135°/α-45°) and (green line, α-45°/α-135°) are extracted from the absorption spectra in Fig. 3(a). The intersection occurs at a wavelength of 397 nm, referring as the reversal point. It should be noted that similar optical reversal phenomenon has also been reported in other low-dimensional materials such as PdSe2,[43] SiP,[44] Ni2Pd3Se8,[45] etc. In Fig. 3(c), the absorption intensities at different angles are compared before and after the reversal point, specifically under 350-nm and 75-nm wavelengths, which observes an approximately 90° distinct reversal. Figure 3(d) displays the polarized light absorption intensity of PdBr2 crystal across a range of polarization angles from 0° to 360°. Notably, there is a clear reversal in polarized light absorption between the 350 nm and 755 nm wavelength ranges. The dichroic ratios at 350 nm and 755 nm are 1.02 and 1.78, respectively, as shown in the inset of Fig. 3(e). Above all, the PdBr2 nanoflake demonstrates a significant linear dichroism effect and an intriguing optical reversal phenomenon, which could be employed for polarization-sensitive photodetection.

    In order to explore the optoelectronic characteristics of PdBr2 nanowire, we build a two-terminal device using an individual PdBr2 nanowire on an SiO2/Si substrate (300 nm in depth). The scheme is illustrated in Fig. 4(a). Figure 4(b) shows the dark field optical microscopy (OM) image of the PdBr2 nanowire device. And the inset of Fig. 4(b) is the bright OM image of the same device. According to previous report,[39] similar device exhibits prominent photoresponse under 405-nm light irradiation. Thus, we primarily study the optoelectrical performances of the photodetector under 405-nm light irradiation. As shown in Fig. 4(c), there is a small Schottky barrier between the electrode and PdBr2 channel material. We also present the Ids–Vds responses using linear coordinates in Fig. S3. The observed asymmetry in the Ids–Vds curves can be attributed to barriers or inherent asymmetries in charge transport. And the photoresponse of PdBr2 nanowire device increases with the increase of Vds under the illumination of different power density. The photocurrent (Iph = Ilight – Idark) increases gradually with increasing of the illuminated power density. The low power density of 0.002 mW⋅mm−2 produces a photocurrent of 1.1 nA at a bias voltage of 3 V, which is about an order of magnitude larger than that under dark condition. Figure 4(d) plots the relationship of Iph with the illuminated power densities (P) at the bias voltage of 3 V. A sublinear photoresponse is observed, and it can be fitted using the power law relation Iph ∝ Pα. Generally, the power exponent α is close to 1, demonstrating the photoconduction mechanism of the photodetector. The presence of a value smaller than 1 may be attributed to the intricate dynamics of carrier generation, trapping, and recombination processes. In the present case, the small value of α = 0.14 suggests that the dominant factor influencing the photocurrent generation in PdBr2 nanowire photodetector is the photogating effect.

    We proceed to calculate the responsivity (R) and detectivity (D*) of the device at 405-nm wavelength using the equations

    where Iph, P, A, e, and Idark are the photocurrent, power density, effective area of the device (∼0.73 μm2), electron charge, and the device current under dark, respectively. The calculated R and D* as the functions of power density are presented in Fig. 4(e). It is found that the responsivity R and detectivity D* can reach 747 A⋅W−1 and 5.8 × 1012 Jones at Vds = 3 V and P = 0.002 mW⋅mm−2, respectively. Figure 4(f) shows the photoresponse speed of the photodetector, where the rise time (τrise) and decay time (τdecay) are defined as the duration time for the photocurrent to increase from 10% to 90% and decrease from 90% to 10%, respectively. The time-resolved photoresponses with 10 cycles observed under periodic illumination at 405-nm wavelength are displayed in Fig. S4. The obtained τrise and τdecay are 0.13 s and 5.19 s, respectively. The longer decay time comparing to the rise time is attributed to the existence of electron–hole trapping states, which prevent the recombination of charge carriers. The presence of trapping states within the material could enhance the photoconductivity of the device. This behavior also confirms that the optoelectronic mechanism in the PdBr2 photodetector device is the photogating effect. We present the wavelength-dependent responsivity of a PdBr2 photodetector covering a range of wavelengths from 405 nm to 940 nm in Fig. S5. It can be found that the responsivity at 405 nm wavelength is remarkably larger than that in other wavelengths, which is attributed to the bandgap and absorption characteristics of PdBr2.

    In view of the intrinsic structural anisotropy of PdBr2, we conduct the study on the anisotropic photoresponses of PdBr2 nanowire photodetector by measuring the polarization-dependent photodetection. Figure 5(a) shows the scheme of the polarized photodetection, where a Glan–Taylor prism and a half-wave plate are utilized to generate linearly polarized light. By switching the on and off state of the laser (405 nm) and synchronously adjusting the polarization angle (θ) of the polarized light from 0° to 360° at a step of 20°, the dynamic photoresponses of the PdBr2 nanowire device are continuously monitored. The photodetector exhibits a periodic photoresponse with a period of 180°. The lowest and highest photocurrents are observed when the light is aligned to be parallel and perpendicular to the a-axis direction of PdBr2 nanowire, respectively. The function Iph = Ipha cos2(θ) + Iphb sin2(θ) provides a good fit for the photocurrent values with respect to polarization angle θ. A high photocurrent anisotropy ratio (Iph–max/Iph–min) of 1.56 has been achieved. The polar diagram in Fig. 5(c) displays the normalized photocurrent distribution. The results indicate a high polarization sensitive photodetector based on PdBr2 nanowire. Figure 5(d) summarizes the wavelength range and the anisotropic ratio of previously reported polarization sensitive photodetectors built of various nanowire and nanobelt materials.[45–56] It is found that the PdBr2 nanowire photodetector exhibits the optimal anisotropic optoelectronic performance at the near-ultraviolet (405 nm) region. The remarkable polarization-sensitive performance of the PdBr2 nanowire photodetector holds great promise for designing multifunctional optoelectronic devices and facilitating their integration and miniaturization.

4.   Conclusion
  • In conclusion, optical reversal of linear dichroism has been established in PdBr2, a quasi-one-dimensional material with in-plane anisotropic structure. The PdBr2 nanowire photodetector exhibits high performance with a responsivity of 746 A⋅W−1 and a detectivity of 5.8 × 1012 Jones, respectively. Moreover, the photodetector demonstrates polarization sensitivity with large photocurrent anisotropy ratio of 1.56. This work demonstrates that PdBr2 can be applied to realize high-performance polarized photodetectors, broadening the application in high sensitivity and polarization-resolved photodetection and imaging applications.

Figure (5)  Reference (61)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return