2024 Volume 33 Issue 6
Article Contents

Shiyue He, Ruoshui Liu, Xujie Liu, Xianping Ye, Lichen Wang, Baogen Shen. Influences of divalent ion substitution on the magnetic and dielectric properties of W-type barium ferrite[J]. Chinese Physics B, 2024, 33(6): 066801. doi: 10.1088/1674-1056/ad39d5
Citation: Shiyue He, Ruoshui Liu, Xujie Liu, Xianping Ye, Lichen Wang, Baogen Shen. Influences of divalent ion substitution on the magnetic and dielectric properties of W-type barium ferrite[J]. Chinese Physics B, 2024, 33(6): 066801. doi: 10.1088/1674-1056/ad39d5

Influences of divalent ion substitution on the magnetic and dielectric properties of W-type barium ferrite

  • Received Date: 17/02/2024
    Accepted Date: 03/04/2024
    Available Online: 01/06/2024
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(6)  /  Tables(3)

Article Metrics

Article views(174) PDF downloads(2) Cited by(0)

Access History

Influences of divalent ion substitution on the magnetic and dielectric properties of W-type barium ferrite

Abstract: Saturation magnetization, magneto-crystalline anisotropy field, and dielectric properties are closely related to microwave devices applied at different frequencies. For regulating the magnetic and dielectric properties of W-type barium ferrites, single-phase BaMe2Fe16O27 (Me = Fe, Mn, Zn, Ni, Co) with different Me ions were synthesized by the high-temperature solid-state method. The saturation magnetization (Ms) range from 47.77 emu/g to 95.34 emu/g and the magnetic anisotropy field (Ha) range from 10700.60 Oe (1 Oe = 79.5775 A⋅m−1) to 13739.57 Oe, depending on the type of cation substitution in the hexagonal lattice. The dielectric permittivity and dielectric loss decrease with increasing frequency of the AC electric field in the low-frequency region, while they almost remain constant in the high-frequency region. The characteristics of easy regulation and preparation make it a potential candidate for use in microwave device applications.

1.   Introduction
  • Hexagonal ferrites, discovered in the 1950s,[1] have been classified into M, W, X, Y, Z, and U types based on the crystal structure.[2] These kinds of materials were found with excellent properties of low electrical conductivity, large saturation magnetization, and outstanding chemical stability, making them an ideal material for applications such as permanent magnets, high-density vertical magnetic recording media, microwave devices and absorption, stealth technology, and multiferroic materials.[3–7] Furthermore, their unique structure and magnetic anisotropy outperform other materials in self-bias high-frequency applications.[8] M-type ferrite has been widely studied due to its simple crystal structure and easy phase formation characteristics. It has become the most well-known and commercially used hard magnet ferrite and is used in microwave devices.[9] However, the regulation of the magnetic performance of M-type ferrite has nearly reached its limitation and makes further rapid improvement very challenging. In contrast, W-type ferrite has almost the same saturation magnetization Ms, more lattice sites than M-type and widely tunable magnetic properties, demonstrating the advantages of W-type hexagonal ferrite in microwave applications.[10–12]

    The chemical formula of W-type ferrite is AMe2Fe16O27 (where A = Sr or Ba, Me = Fe, Mg, Mn, Co, Ni, Cu, Zn). Its crystal structure is similar to that of M-type ferrite. It is composed of spinel blocks (S-blocks) and hexagonal blocks (R-blocks), stacking along the c axis and with the order of RSSR*S*S*. Here * indicates a 180° rotation of the block around the c axis. Figure 1 shows the schematic diagram of the W-type barium ferrite unit cell. The cations occupy seven different lattice sites, including four octahedral sites (12k, 4fVI, 4f, and 6g), two tetrahedral sites (4e and 4fIV), and one trigonal bipyramidal site (2d). Magnetic moments on the 12k, 6g, 4f, and 2d lattice sites align parallel to the c axis (12↑), while those on the 4e, 4fIV, and 4fVI sites align antiparallel to it (6↓).[13]

    Ion substitution is considered an effective method for regulating the magnetic properties of materials and expanding their applications.[14,15] Compared with the M-type ferrites, the crystal sites for cations are more abundant in W-type ferrites, increasing the flexibility of ions occupying appropriate crystal positions. To meet the requirements of various applications, many researchers have attempted to use divalent metal cations to enhance the performance of W-type hexaferrite. Yang et al.[16] prepared Co–Zn co-doped BaW ferrite using the sol–gel method and investigated the microwave absorption, and a maximum loss of −18 dB at 5.5 GHz was reported. SrZnxFe2−xFe16O27 (0 ≤ x ≤ 1.5) were synthesized by the solid-phase method under low oxygen pressure by You et al.,[17] and the results showed that the saturation magnetization was significantly improved. For the x = 1.0 sample that sintered at 1250 °C, the highest Ms value of 87.7 emu/g is obtained. BaZnxCo2−xFe16O27 (x = 0, 0.3, 0.5, 0.7, 0.9, 1.2) was successfully synthesized by chemical co-precipitation by Sun et al.,[18] and the complex permittivity and permeability of the samples were calculated for the determination of the samples in the frequency range of 1 GHz–18 GHz based on the measured data of the microwave vector network analyzer. Ali et al.[19] synthesized Ba0.5Sr0.5Co2–xMexFe16O27 (x = 0, 0.5, Me = Mn, Mg, Zn, Ni) by sol–gel auto-combustion method, and the high saturated magnetization and low coercivity make them promising candidates for microwave absorbing materials. Attia et al.[20] reported the conduction mechanism of BaZn2−xMgxFe16O27 (x = 0.0, 0.4, 0.8, 1.2, and 1.6) prepared by the conventional ceramic method. It is found that these ferrites are n-type semiconductors and their conduction process is mainly a multiple hopping conduction mechanism.

    However, current research on the substitution of Fe ions is relatively scattered and not systematic enough, and the preparation of samples containing Fe2+ ions must be carried out under low oxygen pressure or complex heat treatment, which limits its widespread application. Therefore, in this study, the solid-phase reaction method was used to prepare divalent ion-substituted BaMe2Fe16O2 (Me = Fe, Mn, Zn, Ni, Co) W-type hexagonal ferrite. The effects of different divalent cation substitutions on the magnetic and dielectric properties were analyzed using x-ray diffractometer (XRD), scanning electron microscopy (SEM), Raman, VSM, and LCR meter.

2.   Experiment
  • BaMe2Fe16O27 (Me = Fe, Mn, Zn, Ni, Co) polycrystalline samples were synthesized using the solid-phase reaction method. The starting materials are BaCO3 (Aladdin 99.0% purity), Fe2O3 (Macklin 99.0% purity), ZnO (Alfa Aesar 99.999% purity), MnO (Macklin 99.0% purity), NiO (Macklin 99.0% purity), and Co3O4 (Macklin 99.0% purity). The starting materials were accurately weighted according to stoichiometric ratios, and well mixed in a planetary ball mill (Nanjing Boyuntong Instrument, XGB2) with deionized water at 200 rpm for 2 hours. All the samples were sintered in a regular muffle furnace at 1300 °C for 3 hours, except for the BaFe18O27 sample was sintered in a tube furnace under the protection of a nitrogen atmosphere that can maintain the valence state of Fe2+ ions.[21]

  • The x-ray diffractometer (XRD, Bruker D2 Phaser) equipped with Cu Kα radiation was employed to analyze the phase structure of the synthesized samples, with step size of 0.02° and angular range of 20°–80° (30 kV, 10 mA, λ = 1.54184 Å). The microstructure analysis of the powder was performed using scanning electron microscopy (SEM, Tescan Vega Compact). Raman scattering spectra of all samples were recorded at room temperature using a confocal micro-Raman spectrometer, with laser wavelength of 532 nm and the wavenumber range of 50 cm−1–900 cm−1 (Renishaw inVia Reflex Raman Microscope). The magnetization of the sample was measured at 300 K with the scanning magnetic field range of ±30 kOe (1 Oe = 79.5775 A⋅m−1), by using the vibration sample magnetometer option of physical properties measurement system (Quantum Design, DynaCool Cryogen-free System). The saturation magnetization (Ms) and the magnetic anisotropy field (Ha) were calculated according to the law of approach to saturation. The dielectric properties of the samples were characterized with the Agilent 4980 LCR meter.

3.   Results and discussion
  • Figure 2 depicts the XRD patterns of all BaMe2Fe16O27 (Me = Fe, Mn, Zn, Ni, Co) powder samples collected at room temperature, in which the red lines are the standard BaW ferrite PDF card (PDF#75-0406). The excellent agreement between the observed peaks and the standard patterns indicates that all the samples prepared by the high-temperature solid-state method have single-phase W-type structures. The relative variation of (00l) peak intensity observed in BaFe18O27 sample can attributed to the big size plate-shaped crystalline grain as shown in Fig. 3(a), that can introduce the texture.

  • The magnetic and dielectric properties of W-type hexaferrite are closely related to the microstructure. Figure 3 shows the micrograph of the obtained BaMe2Fe16O27 (Me = Fe, Mn, Zn, Ni, Co) powder sample by using scanning electron microscopy (SEM). All samples have hexagonal plate-shaped grains, consistent with XRD predictions. The images show that the substitution of Fe ions by Me ions leads to significant changes in the grain microstructure, especially for the crystal grain size and the ratio of radius to axis. All samples show large average grain size, that may be due to high sinter temperature and long sinter time. The specific plate-shape structure and larger grain size are favorable for higher frequency application.[4]

  • The crystal structure was further characterized using Raman spectroscopy, which can provide information on the symmetric vibration modes of the crystal and is highly sensitive to the vibrations of atomic bonds. The W-type ferrite exhibits a hexagonal crystal structure with the space group of D6h (P63/mmc). Group theory principles indicate 42 Raman active modes in hexagonal ferrites named as 11A1g+14E1g+17E2g.[22–24] Here, A and E represent symbols for one-dimensional and two-dimensional vibration modes, while g denotes symmetry concerning the center of symmetry.

    The room temperature Raman spectra of BaMe2Fe16O27 (Me = Fe, Mn, Zn, Ni, Co) samples are shown in Fig. 4, which were recorded in the range of 50 cm−1 to 900 cm−1. It is evident that the shape and position of the Raman peaks are affected by the variation of the substituent ion Me2+. In our experiment, Raman spectra analysis revealed ten active modes and these modes with their respective symmetries and associated sites are listed in Table 1. The peaks shown in the figure are all feature Raman peaks of W-type hexagonal ferrite, which are contributed by the vibration of metal–oxygen bonds at different interstitial positions (tetrahedral, octahedral, bipyramidal).[25]

    The main peak at 665 cm−1–672 cm−1 of the Raman spectra, is caused by the vibrations of the bipyramidal (FeO5, 2b site) with A1g symmetry. The vibration modes at 280 cm−1–281 cm−1, 451 cm−1–473 cm−1, 514 cm−1–529 cm−1, and 605 cm−1–614 cm−1 are associated with octahedral (2a, 2a+12k, 12k, and 4fVI sites), respectively, and all exhibit A1g symmetry. The active mode at 174 cm−1–176 cm−1 is due to the entire spinel block vibrations, which have E1g symmetry. The vibrational modes at 324 cm−1–328 cm−1 and 402 cm−1–409 cm−1 can be associated with the octahedra (12k site) and are attributed to E2g and E1g symmetry. In the Me2+ substituted samples, considerable shifts in the Raman characteristic peaks can be found. The substituted ions Mn2+ (0.80 Å), Zn2+ (0.74 Å), Ni2+ (0.72 Å), and Co2+ (0.74 Å) have different ionic radius compares with the host ions Fe3+ (0.64 Å) and Fe2+ (0.76 Å). It can be observed that the peak positions at 672 cm−1 (bipyramidal, FeO5, 2b site) shifted slightly to lower wavelength due to the substitution of Mn2+, Zn2+, and Ni2+. The modes are all reduced in intensity and accompanied by peak broadening. This may be due to the change in ion mass and force constants (based on ion valence states, bond lengths, lattice parameters, etc.) due to substitution.[26] The Raman peak at 614 cm−1 shows a more significant shift and amplitude change in the samples substituted with Me2+, the Mn2+ and Ni2+ substituted samples result in a sharper band. The Raman peak widths are highly sensitive to the substitution of magnetic structures. The maximum change in both substitutions occurs at the octahedral 4fIV site, which may be the factor responsible for these band changes. As the substitution occurs, the peak intensity at 529 cm−1 decreases while the width increases. This is likely due to the local octahedral FeO6 aberration caused by the occupation of the 12k site by the ion with larger radius. These results indicate that the Me2+ ions have successfully entered the BaW sublattice, which may affect the magnetic and dielectric properties.

  • The magnetic hysteresis loops measured for all BaMe2Fe16O27 (Me = Fe, Mn, Zn, Ni, Co) samples at room temperature are depicted in Fig. 5(a). It can be seen that the hysteresis loops exhibit essentially symmetrical “S” shapes. Table 2 summarizes various magnetic parameters extracted from these loops, including saturation magnetization (Ms), coercivity (Hc), and magnetocrystalline anisotropy field (Ha). Values of Ms and Ha are obtained by the M–H curve using the law of approaching saturation.[27] The general expression of this law is

    where Ms represents saturation magnetization, A is the magnetic hardness coefficient, B is the magnetocrystalline anisotropy constant, H denotes the applied magnetic field, and χ is the high-field magnetization susceptibility. In the high field region, the M–1/H2 relationship exhibits linearity, with parameters A and χ becoming very small and negligible. Consequently, the above equation can be simplified to

    For the hexagonal crystal structure with uniaxial anisotropy, B can be expressed as

    Ms and B are calculated from a linear fit to the law of approaching saturation, as shown in Figs. 5(b)–5(f). The magnetocrystalline anisotropy field (Ha) can be derived from Eq. (3). Compared with BaFe18O27, the magnetic measurements reveal that the Ms and Ha decrease with other Me2+ ion doping. This variation in Ms results from the choice of substituent ions in the insertion structure and the occupation of specific cationic sites by Me2+. In W-type hexagonal ferrites, 32 Fe3+ ions and 4 Me2+ ions occupy seven different magnetic sublattices in the unit cell. The distribution and valence states of ions in the lattice contribute differently to the total magnetization intensity, which is determined by the difference between the magnetization intensity at octahedral sites and that at tetrahedral sites. Both Co2+ and Ni2+ ions show a preference for octahedral sites (2a and 12k sites) with spin directions aligned with the overall magnetic moment,[28,29] corresponding to a change in the Raman peak of 521 cm−1 (12k sites). Furthermore, their preference energy for these sites surpasses that of Fe3+ ions. However, since the magnetic moments of the dopant ions Ni2+, Co2+, and Mn2+ (3.0 μB, 4.0 μB, and 2.7 μB, respectively) are smaller than Fe3+ ions (5 μB), the substitution of spin-up Fe3+ ions leads to a decrease in the net magnetization, resulting in a lower saturation magnetization of the sample. The dope of Mn2+ to the W-type hexaferrite weakens the Fe–O–Fe super-exchange interactions, resulting in a decrease in the magnetic properties.[30] Zn2+ is a non-magnetic ion that tends to occupy tetrahedral sites (4e and 4fIV) with spin down.[13,31] Its substitution leads to a weakening of the alignment between the magnetic ions and tilting of the antiparallel alignment of the spins, which results in a reduction of the net magnetic moment. This difference may be due to variations in the evaluation method for the Ms value. The observed low coercivity can be attributed to the overgrowth of crystals at high sintering temperature, which induces a multi-domain character, leading to the disappearance of Hc.[32] Except for the Co2W sample, the variation of the coercivity is in general agreement with the results of the grain size variation derived from the SEM images. In addition, the coercivity is also affected by the anisotropic field. Co2W has planar anisotropy and doping with Co2+ can change the anisotropy of Me2W from c axis to c planar,[33] significantly reducing coercivity. Table 3 lists the properties of similar materials prepared by other researchers, and it can be seen that we have successfully synthesized BaMe2Fe16O27 using a simpler solid-phase reaction method, along with an improvement in coercivity.

  • Figure 6 draws the frequency dependence of the dielectric constant and dielectric loss for the prepared ferrite compounds at room temperature. For all the samples, the dielectric constant and dielectric loss decrease accompanying the frequency range from 100 Hz to 1 MHz. Above 1 MHz, the dielectric permittivity almost remains unchanged. For this phenomenon, it can be attributed to that at low frequencies all the dipole relaxation can well follow the frequency of ac electric field. Therefore, a higher dielectric constant can result. At higher frequencies, however, the electron hopping between Fe3+ and Fe2+ ions lags, and part of the dipoles cannot follow the reversal of field, the samples only present a lower dielectric permittivity finally.[39] By comparing the different compositions of ferrite, it is also found that the Fe2W-ferrite possesses the highest dielectric permittivity, which is similar to Rehman’s report[40] based on Koop’s theory. This could be ascribed to the fact that the Fe cations usually have mixed valence states. It increases the probability of hopping conduction and results in a high value of the dielectric constant. Higher dielectric constants lead to an enhanced skinning effect, which reduces the depth of electromagnetic wave penetration. Therefore, by replacing Fe with other divalent ions, the hopping conduction can be well suppressed. Correspondingly, the dielectric permittivity reduces dramatically, helping their application at high frequencies. Dielectric loss is an important part of the total loss in ferrite cores.[41] Therefore, low dielectric loss is necessary for low core losses. Figure 6(b) shows the dielectric loss as a function of frequency for different compositions. The dielectric loss curve is similar to the real part of the dielectric constant as a function of frequency, which implies that the dielectric properties of ferrite can be adjusted by changing the divalent ions.

4.   Conclusions
  • High purity W-type hexagonal ferrite BaMe2Fe16O27 (Me = Fe, Mn, Zn, Ni, Co) samples with divalent ion substitution were prepared by high-temperature solid-state method, and the structure, magnetic and dielectric properties were systematically investigated. The materials exhibited hexagonal symmetry and belonged to the P63/mmc space group. Raman analysis demonstrated the existence of ten active vibration modes in the wavenumber range of 50 cm−1–900 cm−1. The variations in peak intensity and width of Raman spectra were attributed to changes in ion substitution due to their occupancy. The variations in magnetic properties can be attributed to the magnetic moment and occupancy tendency of the substitute ion itself, and the size of the crystal grain. The dielectric constant and dielectric loss decrease as the frequency increases in the low-frequency region and it becomes a constant in the high-frequency region. Frequency hopping conduction can be well suppressed to achieve dielectric property adjustment by replacing Fe2+ with divalent ions. The magnetic and dielectric properties of BaMe2Fe16O27 are diverse and easily tunable. Therefore, BaW hexaferrite synthesized by substituting Me ions is more conducive to achieve a wider frequency range of applications.

Figure (6)  Table (3) Reference (41)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return