2024 Volume 33 Issue 7
Article Contents

Jing Gong, Huan Wang, Xiao-Ping Ma, Xiang-Yu Zeng, Jun-Fa Lin, Kun Han, Yi-Ting Wang, Tian-Long Xia. Magnetic and electrical transport properties in GdAlSi and SmAlGe[J]. Chinese Physics B, 2024, 33(7): 077302. doi: 10.1088/1674-1056/ad41ba
Citation: Jing Gong, Huan Wang, Xiao-Ping Ma, Xiang-Yu Zeng, Jun-Fa Lin, Kun Han, Yi-Ting Wang, Tian-Long Xia. Magnetic and electrical transport properties in GdAlSi and SmAlGe[J]. Chinese Physics B, 2024, 33(7): 077302. doi: 10.1088/1674-1056/ad41ba

Magnetic and electrical transport properties in GdAlSi and SmAlGe

  • Received Date: 20/03/2024
    Accepted Date: 16/04/2024
    Available Online: 01/06/2024
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(5)  /  Tables(2)

Article Metrics

Article views(406) PDF downloads(6) Cited by(0)

Access History

Magnetic and electrical transport properties in GdAlSi and SmAlGe

Abstract: We conduct a detailed examination of the magnetic and electrical transport properties in GdAlSi and SmAlGe crystals, which possess a LaPtSi-type structure (space group I41md). The magnetic susceptibility data unambiguously reveal magnetic ordering below a characteristic transition temperature (TN). For GdAlSi, a hysteresis loop is observed in the magnetization and magnetoresistance curves within the ab plane when the magnetic field is applied below TN, which is around 32 K. Notable specific heat anomalies are detected at 32 K for GdAlSi and 6 K for SmAlGe, confirming the occurrence of magnetic transitions. In addition, the extracted magnetic entropy at high temperatures is consistent with the theoretical value of Rln(2J + 1) for J = 7/2 in Gd3+ and J = 5/2 in Sm3+, respectively. SmAlGe also exhibits Schottky-like specific heat contributions. Additionally, both GdAlSi and SmAlGe exhibit positive magnetoresistance and a normal Hall effect.

1.   Introduction
  • Recently, the fascinating interplay between electronic correlations and topology has ignited considerable interest in magnetic Weyl semimetals.[1–5] The LnAlX (Ln = rare earth, X = Si, Ge) family offers an excellent platform for investigating their distinctive topological characteristics and rich magnetic properties, which is exemplified by the discovery of pressure-induced superconductivity and a spin Hall effect in LaAlX,[6,7] the observation of anisotropic anomalous Hall effects and a topological magnetic phase in CeAlX,[8–12] the measurement of a significant anomalous Hall conductivity and a field-induced Lifshitz transition in PrAlX,[13–17] and the detection of quantum oscillations, an anomalous Nernst effect, and the formation of helical incommensurate spin density waves in NdAlX.[18–22]

    The insights from earlier research suggest that replacing the rare earth elements in the LnAlX series can lead to a spectrum of magnetic and transport characteristics. This variability spurs our interest in examining the properties of SmAlX and GdAlX. To date, SmAlSi has displayed Shubnikov–de Haas oscillations, topological spiral magnetism, and a Kramers nodal line.[23–27] However, there is a lack of research on the magnetic and electrical transport properties of SmAlGe single crystals. These discoveries solidify our intention to delve deeper into SmAlGe. Concerning GdAlX, GdAlGe exists in a tetragonal phase at temperatures above 1300 K, whereas the orthorhombic phase is formed below this threshold.[28–30] This contrasts with the tetragonal LnAlX family, complicating direct comparisons of their physical properties. To date, only a couple of studies have been published on the tetragonal GdAlSi single crystal,[31,32] highlighting the importance of a more thorough examination of its electronic and magnetic properties.

    In this work, we have successfully grown single crystals of GdAlSi and SmAlGe using the flux method and have conducted a thorough investigation of their magnetic and electrical transport properties. Analysis of powder x-ray diffraction (XRD) patterns from crushed samples confirms that both GdAlSi and SmAlGe crystallize in a noncentrosymmetric structure with the space group I41md. We observe magnetic order below temperatures of 32 K and 6 K for GdAlSi and SmAlGe, respectively. For GdAlSi, we detect a field-induced phase transition with a loop both in magnetization and magnetoresistance (MR) curves. A positive MR, attributed to the Lorentz force, is observed in both GdAlSi and SmAlGe. Furthermore, by analyzing the normal Hall effect, we estimate the carrier concentrations to be approximately ∼ 1.1 × 1021 cm−3 at 2 K for GdAlSi and ∼ 2.5× 1021 cm−3 for SmAlGe. The maximum mobility up to 96 cm2⋅V−1⋅s−1 and 50 cm2⋅V−1⋅s−1 for GdAlSi and SmAlGe are obtained.

2.   Experiment
  • Single crystals of GdAlSi and SmAlGe were grown by the self-flux method. The Gd/Sm ingot, Al column, Si powder and Ge pieces were combined in ratios of Gd : Al : Si = 1 : 10 : 1 and Sm : Al : Ge = 1 : 10 : 1, then placed into an corundum crucible and vacuum sealed in a quartz tube. The quartz tube was placed in a box furnace, which is heated to 1150 °C at a rate of 60 °C/h, and held for two hours. Then, it was cooled to 750 °C with a rate of 3 °C/h, at which the excess Al flux was separated from the crystals by centrifugation. The atomic proportions of GdAlSi and SmAlGe were verified to be Gd : Al : Si = 1 : 1 : 1 and Sm : Al : Ge = 1 : 1 : 1, respectively, using energy dispersive x-ray spectroscopy (EDS, Oxford X-Max 50). The single crystal and powder x-ray diffraction (XRD) data for GdAlSi and SmAlGe were collected from a Bruker D8 Advance x-ray diffractometer using Cu Kα radiation. The refinement of the data was performed using TOPAS-4.2 software. An atomic-resolution high-angle annular dark field (HAADF) image was obtained with a spherical-aberration corrected JEOL ARM200F instrument equipped with double-aberration correctors and operated at 200 kV. The magnetic properties of the samples were measured with a Quantum Design magnetic property measurement system (QD MPMS-3). The electrical resistivity, specific heat, and Hall effect were measured in another Quantum Design physical property measurement system (QD PPMS-14T). Resistivity, magnetoresistance, and Hall resistivity measurement were performed by the four-probe method. To eliminate the influence from voltage probe misalignment, the raw resistivity data were evaluated by the formulae: ρxx(B) = [ρxx(−9 T → 9 T)+ρxx(9 T → −9 T)]/2 and ρxy(B) = [ρxy(−9 T → 9 T)–ρxy(9 T → −9 T)]/2.

3.   Results and discussion
  • As shown in Fig. 1(a), the structure consists of stacks of Gd/Sm, Al, and Si/Ge layers along the c-axis. The single-crystal XRD patterns for GdAlSi and SmAlGe, as shown in the upper panels of Figs. 1(c) and 1(d), respectively, reveal the surface of the samples with the (00l) plane, which is presented in the insets of Figs. 1(c) and 1(d). The powder XRD patterns for GdAlSi and SmAlGe are displayed in the lower panels of Figs. 1(c) and 1(d), respectively, which show no trace of any other impurity phase. From previous reports on LnAlX family, it is now clear that LnAlX family belongs to the noncentrosymmetric space group I41md (No. 109).[8,10,15,20,22,26,31] Subsequently, a refinement of the powder XRD pattern was performed using the space group I41md. The obtained lattice parameters for GdAlSi are a = b = 4.1278 Å, c = 14.4323 Å, and for SmAlGe, they are a = b = 4.1957 Å, c = 14.5880 Å. Table 1 summarizes the refinement parameters for GdAlSi and SmAlGe. The crystal structure of as-grown GdAlSi was further confirmed by the transmission electron microscopy (TEM) data. Figure 1(b) shows an atomically resolved high-angle annular dark-field (HAADF) image of GdAlSi recorded along the [001] zone axis with the corresponding fast Fourier transform (FFT) images inserted. A simulation of the model structure is overlaid with an enlarged image from Fig. 1(b) as shown in the upper-right inset, where Gd, Al, and Si atoms are represented as purple, white, and blue balls, respectively. The lower-right inset presents a typical selected-area electron diffraction (SAED) pattern taken along the [001] zone axis. The diffraction spots can be well indexed with respect to the space group I41md, with a = b = 4.08 Å, which is consistent with the result obtained from XRD measurement.

  • Figures 2(a) and 2(b) show the temperature dependence of longitudinal resistivity (ρxx) for GdAlSi and SmAlGe, respectively, which indicates typical metallic behavior. It can be seen that the resistivity shows a kink at 32 K for GdAlSi, indicating the Néel temperature, and this is also evidenced in the specific heat [Fig. 2(c)]. The magnetic phase transition temperature is consistent with previous reports.[31,32] In general, a kink or drop on resistivity curve may happen related to transitions. However, in the magnetic SmAlGe, the interaction between the electrons and spin may be too weak and no kink or drop is observed at TN in the resistivity. Similar behavior has also been reported in MnSb6Te10[33] and Eu3In2P4,[34] etc.

    The measurement of specific heat is a valuable technique for investigating magnetic ordering phenomena in materials. It not only indicates the magnetic ordering temperature but can also be employed to estimate the magnetic entropy, which, in turn, can provide information about crystalline electric field (CEF). The specific heat of GdAlSi and SmAlGe, as well as their nonmagnetic isostructural LaAlSi and LaAlGe, in zero magnetic field is presented in Figs. 2(c) and 2(d). As the temperature decreases, a peak emerge around 32 K for GdAlSi and 6 K for SmAlGe, indicating the emergence of magnetic phase transition. In contrast, the specific heat of LaAlSi and LaAlGe exhibits no anomalies, which is consistent with that expected for nonmagnetic reference compounds.

    The magnetic contribution of GdAlSi and SmAlGe to specific heat Cm are calculated by subtracting the data of isostructural non-magnetic LaAlSi and LaAlGe CLa, as shown in the inset of Figs. 2(c) and 2(d). The sharp peaks observed around 32 K in GdAlSi and 6 K in SmAlGe are indicative of magnetic phase transitions. Figure 2(d) shows a broad peak around 26 K, which is related to the Schottky anomaly contributed by the CEF splitting of Sm3+ atomic levels. This behavior of the specific heat has also been observed in CeAlSi,[8] NdAlSi,[18,22] and SmAlSi.[26] The Schottky specific heat Csh of two levels is estimated using the equation[35]

    where n is the number of Sm atom in one formula, R is the gas constant, Δ is the energy separation between the lowest and first excited states measured in K, and g0/g1 is the degeneracy ratio between the ground state and the excited state. For SmAlGe, the parameters used are n = 1 and g0/g1 = 1/2, respectively. The Schottky fits (carmine dashed line) yield a CEF gap Δ = 6.1 meV in SmAlGe. Because the Gd3+ ion has a zero orbital magnetic moment (L = 0),[36–38] the crystal field splitting is negligible, resulting in no Schokkty anomaly observed in GdAlSi. To examine the energy spectrum of the CEF states, the magnetic entropy Sm(T) is calculated according to the equation

    and plotted in the insets of Figs. 2(c) and 2(d). The magnetic entropy saturates around 100 K at value of 16 J⋅mol−1⋅K−1 and 14 J⋅mol−1⋅K−1 for GdAlSi and SmAlGe, which is close to Rln (2J + 1) = R ln 8 and R ln 6 expect for J(Gd3+) = 7/2 and J(Sm3+) = 5/2, respectively.

  • Figures 3(a) and 3(c) show the temperature-dependent magnetic susceptibilities χ(T) with H ∥ c and H ∥ ab under the zero-field-cooled (ZFC) and field-cooled (FC) modes for GdAlSi and SmAlGe, respectively. With H ∥ ab, the ZFC and FC curves show a kink at 32 K in GdAlSi, which marks the onset of magnetic order. As the temperature further decreases, the ZFC and FC curves do not saturate, as shown in the inset of Fig. 3(a). With H ∥ c, ZFC and FC nearly saturate at low temperature with slight bifurcation. As we measured χ(T) at 50 Oe, it differs from the previously reported results at 1000 Oe.[31] For SmAlGe, with H ∥ ab, as the temperature decreases, the ZFC and FC curves bifurcate and begin to drop at 6 K, which marks the onset of magnetic order as shown in the inset of Fig. 3(c). With H ∥ c, the ZFC and FC curves slightly bifurcate around 6 K and do not saturate at 2 K.

    Figure 3(b) shows the inverse magnetic susceptibility 1/χ curve fitted by the Curie–Weiss law expression between 50 K to 300 K for GdAlSi,

    where C is the Curie constant, and θ is the Weiss temperature. From the fitting of Eq. (3), θab = −102 K and θc = −151 K are obtained, which indicates the dominant AFM interaction for GdAlSi. The C is 8.9 emu⋅K⋅mol−1⋅Oe−1 (H ∥ ab) and 14.4 emu⋅K⋅mol−1⋅Oe−1 (H ∥ c). The effective magnetic moments along different directions are estimated with relation μeff=8C. The yielding effective magnetic moment is 8.4 μB with H ∥ ab, which approaches to the theoretical value of a free Gd3+ ion, which is approximately 7.9 μB. With H ∥ c, the effective moment is determined to be 10.7 μB, which is larger than the theoretical value of a free Gd3+ ion. The surplus moment may be attributed to the conduction electron spin polarization.[39–42]

    A significant curvature of inverse magnetic susceptibility (1/χ) occurs in SmAlGe [Fig. 3(d)], which is usually observed in metallic rare earth magnets due to a large Pauli contribution to the susceptibility.[43] In this case, the curve can be described by a modified Curie–Weiss law within the temperature range of 25 K to 300 K,

    where χ0 is the temperature-independent term including the contribution from the core diamagnetism and the Van Vleck paramagnetism. From the fitting of Eq. (4), θab = −3.01 K and θc = −7.79 K are obtained, which indicates the dominant AFM interaction in SmAlGe. The C is 0.13 emu⋅K⋅mol−1⋅Oe−1 (H ∥ ab) and 0.15 emu⋅K⋅mol−1⋅Oe−1 (H ∥ c). The effective magnetic moment approaches 1.0 μB both in the ab plane and along the c-axis, which approaches the theoretical value of a free Sm3+ ion (∼ 0.85 μB). The parameters obtained from Eqs. (3) and (4) of the χ−1(T) data are summarized in Table 2.

    Isothermal M(H) curves with H applied parallel to the ab plane and along the c-axis in GdAlSi are shown in Figs. 4(a) and 4(c). The magnetization curves are linear at high temperatures, which corresponds to the paramagnetic state. A hysteresis behavior in low field occurs to each M(H) curve below TN, which may implies a field-induced phase transition.[6,24,26,44] With the temperature decreases, the hysteretic metamagnetic transition shifts to lower fields. The dM/dH as a function of field is shown in Fig. 4(b). The magnetizations are discovered to keep increasing as field increases and do not reach saturation at 2 K. The maximum moment approximately 0.77 μB/Gd with H ∥ ab, as shown in the inset of Fig. 4(a). With H ∥ c, the magnetization does not show any signature of saturation up to a field of 7 T at 2 K, and attains a value of only 0.75 μB/Gd as shown in Fig. 4(c), which confirms the antiferromagnetic ordering of the Gd moments.

    The magnetization of SmAlGe as a function of field at different temperatures with H ∥ ab and H ∥ c is shown in Fig. 4(d). The magnetization curves are linear at high temperatures above TN, which corresponds to the paramagnetic state. With the temperature decreasing, the moments with H ∥ ab gradually increase and a small hysteresis loop appears around zero field, which corresponds to the bifurcation behavior of the χ–T curve. At 2 K, the magnetization exhibits a continuous increase until the field reached 7 T. The maximum moment of ∼ 0.09 μB/Sm with H ∥ ab. With H ∥ c, the magnetization also does not show any signature of saturation up to a field of 7 T at 1.8 K and attains a value of only 0.09 μB/Sm, as shown in the inset of Fig. 4(d).

  • To investigate magnetotransport of GdAlSi, the field dependent MR are measured with H ∥ ab and H ∥ c, as shown in Figs. 5(a) and 5(c), in which the MR is defined as [ρxx(μ0H) – ρxx(0)]/ρxx(0). Positive MRs are observed with H ∥ ab and H ∥ c, which is due to the scattering of the conduction electrons in cyclotron motion of the carriers influenced by Lorentz force in magnetic field.[45] With H ∥ ab, hysteresis loops are observed at finite fields below 30 K, possibly due to metamagnetic transitions.[44,46] With the temperature decreases, the hysteresis loop shifts to lower field. This behavior is consistent with the M(H) curve. Meanwhile, we measured the angular MR, with the field directed at various angles (θ) with respect to the c-axis in the yz plane at 2 K, as depicted in Fig. 5(b). The schematic diagrams of experimental setup are shown in the inset of Fig. 5(b). The MR values increase with the applied field and do not saturate until 14 T. Figure 5(e) exhibits the field dependence of ρxx at 2 K (below TN ∼ 6 K) and 8 K (above TN ∼ 6 K) for SmAlGe. The measurement configuration is shown in the inset of Fig. 5(e).

    The field dependence of Hall resistivity of GdAlSi and SmAlGe at various temperatures are measured, as shown in Figs. 5(c), 5(d), and 5(f). The positive sign of Hall coefficient indicates that the charge carriers are hole-type in both GdAlSi and SmAlGe. The insets of Figs. 5(d) and 5(f) show carrier concentrations n and mobilities μ as a function of temperature. Using the one-band model, the carrier concentration is estimated to be ∼ 1.1 × 1021 cm−3 and ∼ 2.5× 1021 cm−3 at 2 K for GdAlSi and SmAlGe, respectively. The carrier concentrations in the LnAlSi family of compounds are higher than those in other compounds within the same family.[13,18,23,24,31] The mobilities of GdAlSi and SmAlGe equals 96 cm2⋅V−1⋅s−1 and 50 cm2⋅V−1⋅s−1 using μ = 1/(enρ(0T)) as shown in the insets of Figs. 5(d) and 5(f).

4.   Conclusion
  • In summary, we have systematically investigated the magnetic and electrical transport properties of GdAlSi and SmAlGe, which have a LaPtSi-type structure (space group I41md). The magnetic phase transitions occur at 32 K for GdAlSi and at 6 K for SmAlGe, respectively. The results of the Curie–Weiss fitting indicate the presence of AFM interactions in both GdAlSi and SmAlGe. Additionally, GdAlSi exhibits a field-induced phase transition in magnetization and MR. The normal Hall effect is observed in both GdAlSi and SmAlGe. The carrier concentration at 2 K is ∼ 1.1× 1021 cm−3 and the mobility is 96 cm2⋅V−1⋅s−1 for GdAlSi, while for SmAlGe, the carrier concentration is approximately 2.5 × 1021 cm−3 and the mobility is 50 cm2⋅V−1⋅s−1. These findings not only provide a new platform for studying the transport properties of the LnAlX (Ln = rare earth; X = Si, Ge) family but also deepen our understanding of the exotic physical phenomena associated with magnetic properties.

Figure (5)  Table (2) Reference (46)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return