2024 Volume 33 Issue 11
Article Contents

Jia-Hong Li, Qing-Li Zhang, Gui-Hua Sun, Jin-Yun Gao, Ren-Qin Dou, Xiao-Fei Wang, Shou-Jun Ding. Crystal growth, structure and crystal field splitting and fitting of Yb:GdScO3[J]. Chinese Physics B, 2024, 33(11): 117601. doi: 10.1088/1674-1056/ad72d3
Citation: Jia-Hong Li, Qing-Li Zhang, Gui-Hua Sun, Jin-Yun Gao, Ren-Qin Dou, Xiao-Fei Wang, Shou-Jun Ding. Crystal growth, structure and crystal field splitting and fitting of Yb:GdScO3[J]. Chinese Physics B, 2024, 33(11): 117601. doi: 10.1088/1674-1056/ad72d3

Crystal growth, structure and crystal field splitting and fitting of Yb:GdScO3

  • Received Date: 17/06/2024
    Accepted Date: 22/08/2024
    Available Online: 01/11/2024
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(5)  /  Tables(4)

Article Metrics

Article views(491) PDF downloads(0) Cited by(0)

Access History

Crystal growth, structure and crystal field splitting and fitting of Yb:GdScO3

Abstract: A good quality (5 at.% Yb:GdScO3) single crystal of Φ30 mm × 37 mm was grown successfully by the Czochralski method. Its structure is studied by the x-ray diffraction (XRD), and its atomic coordinates are obtained by Rietveld refinement. The crystal field energy level splitting of Yb3+ in GdScO3 is determined by employing the absorption and photoluminescence spectra at 8 K. Only 2F7/2(4) is far from the ground state 2F7/2(1) by 710 cm−1 among the crystal field energy levels split from 2F7/2, so it is more easier to realize the laser operation of 2F5/2(1)→2F7/2(4) with wavelength 1060 nm. The spin–orbit coupling parameters and intrinsic crystal field parameters (CFPs). The intrinsic crystal field parameters B¯k (k = 2, 4, 6) of the crystal were fitted by the superposition model. The CFPs evaluated with B¯k and coordination factor are taken as the initial parameters to fit the crystal field energy levels of the crystal, and the crystal field parameters Bqk are obtained finally with the root-mean-square deviation 9 cm−1. It is suggested that the ligand point charge, covalency and overlap interaction are slightly weaker than charge interpenetration and coulomb exchange interaction for Yb3+ in GdScO3. The obtained Hamiltonian parameters can be used to calculate crystal field energy levels and wave functions of Yb:GdScO3 to analyze the mechanism of the luminescence or laser.

1.   Introduction
  • Rare-earth scandate crystals (REScO3, RE = rare earth ions) are promising candidates to replace SiO2 in Si-based metal-oxide-semiconductor field effect transistors (MOSFETs) because of their high dielectric constants, high proton conductivity, large optical band gaps (> 5.5 eV) and good thermodynamic stability compared to silicon.[1–9] Rare earth scandium is ferroelastic, as opposed to LaAlO3 or BaTiO3 substrates, and growth of ferroelastic domains is a unique advantage of existing rare earth scandate substrates. It is mainly used in epitaxial growth of multiferroic, ferroelectric and superconducting perovskite materials. Understanding of functional ABO3 perovskite-type oxides is an active research area with relevance to both fundamental and application-related issues.[10–17] A special aspect of perovskite is its ability to incorporate almost all elements in the periodic table into its structure, resulting in a large number of observed structural distortions, which in turn lead to an extraordinary abundance of physical properties in the perovskite family.[18]

    Gadolinium scandate (GdScO3) crystal is perovskite structure (GdFeO3 type) and belongs to an orthorhombic system with space group of Pnma (No. 62). This crystal is a promising efficient laser host and can be grown by the conventional Czochralski method.[19–25] Firstly, GdScO3 crystal has stable chemical properties, high thermal conductivity and excellent mechanical properties. Secondly, the site symmetry of Gd3+ is low, which is beneficial to removing the parity transition prohibition in 4f configuration of rare earth ions and improving the luminescence efficiency. Thirdly, the crystal has large birefringence effect. When pumped by a high power laser diode, its natural birefringence is much larger than thermal birefringence and dominant, which can eliminate the adverse effects caused by thermal birefringence such as thermal depolarization loss.[26] Lastly, the crystal has a lower phonon energy of 452 cm−1 in comparison with other oxide crystals, such as YAG (860 cm−1), which is beneficial to reduce the probability of multi-phonon relaxation.[27–31]

    Yb3+ has a typical f–f transition with good luminescence characteristics, which has ground multiple state 2F7/2 and excited multiple state 2F5/2 with the interval of about 10000 cm−1.[32] It has no excited state absorption, upconversion and cross relaxation, resulting in the high efficiency and low thermal load during the laser operation.[33–40] In addition, its broad absorption band from f–f transition matches well with the emission wavelength of 900–1000 nm of commercial InGaAs laser diodes (LDs), which make it possible to develop high power solid state laser.[41–44] It has been reported that Yb:GdScO3 is a high-efficiency laser material and it achieved 13.45 W continuous laser output at 1063.9 nm.[45] However, its structure, crystal field splitting and Hamiltonian parameters have not been reported. In this work, 5 at.% Yb:GdScO3 single crystal was grown by the Czochralski method and its structure is determined by Rietveld refinement to its x-ray diffraction (XRD). Crystal filed energy splitting of Yb3+ in GdScO3 host is obtained with the photoluminescence and absorption spectra at the low temperature. In addition, Hamiltonian parameters of Yb3+ in the crystal is fitted, which can be used to investigate the luminescence mechanism such as optical transition probability.

2.   Experiment
  • In the experiment, 5 at.%Yb:GdScO3 single crystal was grown by employing the Czochralski method with an Ir crucible in N2 atmosphere. Raw materials are Sc2O3 (99.9995%), Gd2O3 (99.995%), and Yb2O3 (99.995%). The raw materials were weighted with the following stoichiometric ratio:

    where x = 0.05. The raw materials were mixed thoroughly. In order to reduce the volume of the raw materials, the mixture was pressed into disks of about Φ55 mm × 20 mm, and calcined at 1250 °C in a box furnace for 24 h in atmosphere to form polycrystalline through solid state reaction. After calcination, the polycrystalline disks were taken out and loaded into an iridium crucible of Φ60 mm × 60 mm for crystal growth in a Czochralski furnace JGD80, made in the 26th Institute of CETC. After thermal insulators and single crystal seed with 〈100〉 orientation were installed, the furnace was cleaned, closed and vacuumed up to 1–10 Pa, then nitrogen was filled to protect iridium curable from oxidation during crystal growth. Then the material is heated by intermediate frequency induction supply. After the material is completely melted, the seed crystal is dipped into melt slowly when the melt surface center temperature was adjusted to the melt point of GdScO3 melt, then pulled up with pull rate of 0.2–0.8 mm/h and rotating rate of 5–10 rpm. Crystal growth control software is CZControl XE, developed by Anhui Institute of Optics and Fine Mechanics of CAS, were used to grow it. The obtained boule diameter and length of Yb:GdScO3 crystal are 30 mm and 37 mm, respectively, as shown in Fig. 1.

  • A crystal disk was cut from the as-grown crystal and ground into powder for powder x-ray diffraction (XRD) measurement. The powder XRD measurement was carried out at room temperature with the X’pert Pro XRD of Philips company in the Netherlands. The x-ray was Cu Kα radiation, the tube voltage and current were 40 kV and 40 mA, respectively. The scanning mode was continuous scanning mode with scanning step of 0.033°, and scanning range of 10°–90°. In order to obtain good-resolution emission spectra to determine crystal field splitting, the emission spectra of the crystal were measured under the excitation of 940 nm LD by Edinburgh FLSP-920 spectrometer at temperature 8 K. The absorption spectrum of Yb:GdScO3 crystal was measured by PE Lambda 950 spectrophotometer in the range of 250–3000 nm at temperature of 8 K.

3.   Results and discussion
  • The as-grown Yb:GdScO3 crystal is shown in Fig. 1. It is light yellow and smooth on its surface. The whole crystal is transparent and crack-free.

    The powder x-ray diffraction of Yb:GdScO3 is shown in Fig. 2. Because of the same chemical valence and similar ion radius (the radius of Yb3+ is 0.0985 nm, Gd3+ is 0.1053 nm, and the coordination number of Gd3+/Yb3+ is 8), Gd3+ is easily replaced by Yb3+. Rietveld refinement was performed to its XRD with software package GSAS. The lattice parameters, atomic coordinates, and temperature factors of Yb3+:GdScO3 were refined. The refined residuals RP and RWP are 3.48% and 4.71%, respectively, which means that the calculated results are in good agreement with the experimental data. The fitted results are shown in Fig. 2, and the structural parameters are listed in Table 1. The cell parameters are fitted to be a = 0.5734355 nm, b = 0.7912412 nm, c = 0.5467406 nm, and α = β = γ = 90°. The cell volume is V = 0.248052180 nm3 and the calculated crystal density is ρ = 6.701 g⋅cm−3. The unit cell parameters of GdScO3 are a = 0.5750224 nm, b = 0.7936361 nm, c = 0.5485421 nm, and the unit cell volume V = 0.250331367 nm3. It can be seen that the parameters and cell volume of Yb:GdScO3 decrease slightly.

  • In order to describe crystal field splitting of Yb3+ in GdScO3, the crystal field energy levels split from term 2F5/2 are labeled as 2F5/2(1), 2F5/2(2) and 2F5/2(3), from term 2F7/2 are labeled as 2F7/2(1), 2F7/2(2), 2F7/2(3) and 2F7/2(4) from the low to high energy, respectively.

    The absorption spectrum of Yb3+:GdScO3 at 8 K is shown in Fig. 3. Three absorption peaks at 924.2 nm, 957.2 nm and 984.8 nm are corresponding to the transitions 2F7/2(1)→2F5/2(1), 2F7/2(1)→2F5/2(2) and 2F7/2(1)→2F5/2(3) respectively. Therefore, the corresponding energy levels of 2F5/2(3), 2F5/2(2) and 2F5/2(1) are 10820 cm−1, 10447 cm−1 and 10154 cm−1, respectively.

    The emission spectrum of Yb3+:GdScO3 excited by 940 nm at 8 K is shown in Fig. 4. It can be observed that there exists a strong emission peak at 997.7 nm. The emission spectrum can be fitted by eleven Lorentz peaks, which are 968.7 nm, 988.1 nm, 993.0 nm, 994.7 nm, 997.7 nm, 992.2 nm, 1004.7 nm, 1009.4 nm, 1026.8 nm, 1033.6 nm, and 1058.8 nm, respectively. The emission peaks at 986.7 nm, 997.7 nm, 1026.8 nm and 1058.8 nm are corresponding to the transition energies of 10135 cm−1, 10023.1 cm−1, 9739 cm−1, and 9445 cm−1, respectively. Because the energy gaps among crystal field energy levels split from 2F5/2 are very small (less than or nearly equal to the phonon energy), the photoluminescence transition from 2F5/2(3) and 2F5/2(2) cannot be observed due to rapid phonon relaxation process to the lowest crystal field split energy 2F5/2(1). The sharp peak at 997.7 nm should be assigned to the transition between the lowest crystal field energy level 2F5/2(1) and 2F7/2(2). The transition energy of 997.7 nm is 10023.1 cm−1, so the energy level position of 2F7/2(2) should be 131 cm−1. The emission peaks at 1026.8 nm and 1058.8 nm, whose transition energies are 9739 cm−1 and 9444.7 cm−1, should be attributed to the higher and highest crystal field levels of 2F7/2, which are labeled as 2F7/2(3) and 2F7/2(4), and their energy position can be determined to be 415 cm−1 and 710 cm−1, respectively.

    In a word, the crystal energy splittings of Yb3+:GdScO3 are 10154 cm−1, 10447 cm−1, 10820 cm−1 for 2F5/2, and 0 cm−1, 131 cm−1, 415 cm−1, 710 cm−1 for 2F7/2. The energy level splitting of Yb3+:GdScO3 is shown in Fig. 5. The energy level splitting is slightly smaller than that of Yb:YAG (2F5/2: 10930 cm−1, 10624 cm−1, 10327 cm−1; 2F7/2: 0 cm−1, 564 cm−1, 606 cm−1, 787 cm−1).[46]

    The crystal field energy level structure of 2F7/2 can affect the population inversion property greatly. It is helpful to compare it with Yb:YAG. The crystal energy splittings of 2F7/2 in Yb:YAG are 0 cm−1, 564 cm−1, 606 cm−1 and 787 cm−1. It can be seen that the energies of 2F7/2(2), 2F7/2(3), 2F7/2(4) are much higher than those of 2F7/2(1), which means that it is easier to realize the population inversion of 2F5/2(1)→2F7/2(2), 2F7/2(3) and 2F7/2(4) during laser operation. For Yb:GdScO3, 2F7/2(2) and 2F7/2(3) are closer to the ground state 2F7/2(1), so it is difficult to realize population inversion, and it is more easier to realize the laser operation from 2F5/2(1)→2F7/2(4) with wavelength around 1060 nm.

  • The crystal field at a magnetic ion can be expressed as a simple sum of separate contributions from each of the ligand ions by superposition mode,[47] and crystal field parameter Bqk calculated by intrinsic crystal field parameter B¯k(R0), ligand factor gk,q(θL, ϕL), and power tk (usually tk is taken as k + 1),

    where R0 is the shortest distance between the magnetic ion and all of ligands, RL represents the distance of the L-th ligand, θL and ϕL are the angular position of the L-th ligand.[47]

    The electronic configuration of Yb3+ is f13, and its conjugate state is f1. The Hamiltonian in GdScO3 can be expressed as

    where Eav is the kinetic energy of f electrons and the Coulomb interaction between them and the electrons in the nucleus and full shell, and the second term stands for spin–orbit coupling, ss and ll are spin and angular momentum operators of i-th f electron, ζ is the spin–orbit coupling parameter. The third term stands for the crystal field interaction, Bqk is the crystal field parameter, and Cqk is the angular partial operator of the crystal field. The site symmetry is mirror symmetry m or Cs normal to the orientation [010], a transformation operation M is applied on X = (x,y,z)T to get X′ = (x′,y′,z′)T so that the normal orientation of mirror symmetry is [001],

    The origin of X and X′ is the site of Gd/Yb.

    For Cs symmetry of Yb3+ replacing Gd3+ in GdScO3, the (k, q) values of non-vanished Bqk can be taken as (2, ±2), (2, 0), (4, ±4), (4, ±2), (4, 0), (6, ±6), (6, ±4), (6, ±2), and (6, 0). Three B0k values are real, six B0k(q≠0) values are complex with 12 real variables, and there are 15 independent crystal field parameters totally.

    In order to obtain the Hamiltonian parameters, firstly, the Hamiltonian matrix elements of Yb3+ in GdScO3 were calculated in the space spanned by the base vectors |f13SLJM〉 of Yb3+, where S = 1/2, L = 3, J = 7/2 and 5/2; M = ±7/2, ±5/2, ±3/2, ±3/2 when J = 7/2; M = ±5/2, ±3/2, ±3/2 when J = 5/2. Secondly, three intrinsic crystal field parameters B¯k (k = 2,4,6) were fitted to the energy levels obtained from absorption and emission transitions. Thirdly, the initial crystal filed parameters Bqk were calculated from the intrinsic B¯k obtained in step 2 and coordination factors, and would be used as initial values to fit the experimental energy levels,[46–49] in which the energy derivative is calculated by[46–49]

    where Pi is the i-th Hamiltonian parameter, and Oi is the matrix corresponding to the i-th Hamiltonian parameter, D stands for the matrix diagonalization to obtain eigenvalue; ε is a very small quantity. The final step of D operation is to rearrange eigenvalues from the lowest priority to the highest.

    The fitting parameters of the superposition model include Eav, ζ, B¯2, B¯4, and B¯6, whose initial values are 0 cm−1, 2900 cm−1, 200 cm−1, 200 cm−1, and 200 cm−1, respectively. If the principal of m symmetry is [010], all of Bqk computed from coordination factor gk,q are real, and only B0k will be real and Bqk(q≠0) will be complex if the site symmetry principal axis is in the direction of [001]. The fitting error is smaller when the principal axis is [010], so the intrinsic crystal parameters were fitted under the principal axis [010] of Cs symmetry. The fitting results are insensitive to the initial values of B¯2, B¯4 and B¯6, which indicates that the fitting is reasonable. The orthogonal coordinates of coordination oxygen are shown in Table 2, which is used to calculate coordination factor gk,q. After 19 iterations, the root-mean-square deviation σ is 27 cm−1 [σ=∑i(Eexp,i−Ecal,i)2/N], where Eexp,i and Ecal,i stand for the i-th experimental and calculated energy levels, N is total number of fitted energy levels, and the relative residual factor R is 0.31%. The obtained Hamiltonian parameters Eav, ζ, B¯2, B¯4, and B¯6 are 4668, 2899, −4812, 3681, and −637 in cm−1, respectively. The crystal field parameters Bqk computed from B¯k and coordination factor gk,q with principal axis [010] and [001] are listed in Table 4. Bqk with symmetry axis [001] were used as the initial parameters for further energy level fitting, where Eav, ζ and Bqk are variable. After 16 iterations, the root-mean-square deviation σ is 9 cm−1, the relative residual factor R is 0.6%. The calculated and experimental energy levels are consistent very well with each other, and the final crystal filed parameters are listed in Table 3.

    It can be seen that B06 changes from −87 cm−1 to 155 cm−1, B44 from (26+232I) cm−1 to (−5+455) cm−1, B26 from (45–29I) cm−1 to (−42−114I) cm−1, the signs of the other Bqk are the same as those computed from B¯k. Based on this case, the real parameters Bqk computed with B¯k of symmetry axis [010] were used to analyzed further, among which, except B02, B24 and B46 with positive values, the other Bqk are negative and the absolute maximal value is 1566 cm−1, which indicates that the ligand point charge, covalency and overlap interaction are slightly weaker than charge interpenetration and Coulomb exchange. The Bqk values of Yb:YAG have also been listed in Table 4, only B02, B66 and B26 are negative among nine crystal field parameters, the others are positive, indicating that the ligand point charge, covalency and overlap interaction are important in YAG.

4.   Conclusion and perspectives
  • In this work, (5 at.%)Yb:GdScO3 single crystal is grown by the Czochralski method, its structure parameters are fitted to XRD by Rietveld refinement, the unit cell parameters and atomic coordinates are obtained. Its crystal filed energy level splitting of Yb:GdScO3 is determined by the absorption and photoluminescence spectra at 8 K. Among its crystal field energy levels from 2F7/2, only 2F7/2(4) is far from the ground state 2F7/2(1) by 710 cm−1, so it is more easier to realize the laser operation of 2F5/2(1)→2F7/2(4). The spin–orbital coupling parameters, intrinsic crystal field parameters, and crystal field parameters of Yb:GdScO3 are fitted to its crystal field energy splitting. Bqk of the symmetry principal [010] indicates that the ligand point charge, covalency and overlap interaction are slightly weaker than charge interpenetration and coulomb exchange for Yb3+ in GdScO3, which is in contrary to Yb:YAG.

Figure (5)  Table (4) Reference (49)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return