2024 Volume 33 Issue 12
Article Contents

Yuyang Jiang, Cuiying Pei, Qi Wang, Juefei Wu, Lili Zhang, Chao Xiong, Yanpeng Qi. Pressure-induced superconductivity and phase transition in PbSe and PbTe[J]. Chinese Physics B, 2024, 33(12): 126105. doi: 10.1088/1674-1056/ad8ecc
Citation: Yuyang Jiang, Cuiying Pei, Qi Wang, Juefei Wu, Lili Zhang, Chao Xiong, Yanpeng Qi. Pressure-induced superconductivity and phase transition in PbSe and PbTe[J]. Chinese Physics B, 2024, 33(12): 126105. doi: 10.1088/1674-1056/ad8ecc

Pressure-induced superconductivity and phase transition in PbSe and PbTe

  • Received Date: 29/09/2024
    Accepted Date: 01/11/2024
    Available Online: 01/12/2024
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(7)  /  Tables(1)

Article Metrics

Article views(727) PDF downloads(9) Cited by(0)

Access History

Pressure-induced superconductivity and phase transition in PbSe and PbTe

Abstract: The IV–VI semiconducting chalcogenides are a large material family with distinct physical behavior. Here, we systematically investigate the effect of pressure on the electronic and crystal structures of PbSe and PbTe by combining high-pressure electrical transport and synchrotron x-ray diffraction (XRD) measurements. The resistivity of PbSe and PbTe changes dramatically under high pressure and a non-monotonic evolution of ρ(T) is observed. Both PbSe and PbTe are found to undergo semiconductor–metal transition upon compression and show superconductivity under higher pressure. The structural evolutions from the Fm3¯m to Pnma phase and then to the Pm3¯m phase in PbSe are verified by the x-ray diffraction. The present findings reveal the internal correlation between the structural evolution and the physical properties in lead chalcogenides.

1.   Introduction
  • The IV–VI semiconductors MX (M = Ge, Sn, Pb; X = S, Se, Te) have been extensively investigated for many years because of their various physical properties and technological applications.[1–3] Among them, PbX materials were well known for high carrier mobility as well as high ZT value in mid-temperature region thus gained wide applications in solar cells and thermoelectric field.[4,5] Germanium chalcogenides, like GeSe and GeTe, known as phase-change materials, have been used as data storage devices.[6,7] From structure point of view, the IV–VI semiconductors crystallize in three different structures under ambient conditions.[8] The GeS type structure analogous to black phosphorus is observed for the lighter compounds GeS, GeSe, SnS and SnSe. Compounds SnTe, PbS, PbSe and PbTe crystallize with the cubic NaCl structure, and GeTe shows a rhombohedral structure as a binary analogue of the gray arsenic.

    Pressure, serving as a key thermodynamic parameter, offers a potent means to manipulate crystal and electronic band structures without introducing impurities or defects, thereby unveiling novel physical phenomena that are not observable under ambient conditions.[9–16] As one of the most significant features of the IV–VI compounds, complex structural transitions are observed upon compression.[7,17–25] Initial GeS-type compounds, like SnS and SnSe, undergo two pressure-induced structural transitions: the first from orthorhombic GeS-type structure (space group Pnma) to orthorhombic structure (space group Cmcm) and then to cubic CsCl-type structure (space group Pm3¯m).[19,26,27] PbX (X = Se, Te) and other NaCl-type IV–VI compounds experience a similar evolution path: first from the rocksalt NaCl structure (space group Fm3¯m) to a lower symmetrical phase (space group Pnma) and then to body-centered cubic CsCl structure (space group Pm3¯m).[8,28] Specially, it has been theoretically predicted by Barone et al. that external pressure can induce topological phase transitions in PbSe and PbTe within a rocksalt structure.[29]

    Another typical phenomenon for the IV–VI compounds under high pressure is the semiconductor–metal transition presented along with the phase transformation.[9,17,18,26,27,30] As pressure increases, a huge reduction of the resistivity emerges and compounds finally enter metallic state. The exact structural evolution with pressure for the IV–VI compounds has been clarified, however, the origin of anomaly in resistivity curve still remains unknown. With many of these compounds, superconductivity was only reported in the 1970s and 1980s,[31–33] it is important to examine the relationship between their electronic transition as well as superconducting properties and the structural transformation under high pressure. Motivated by the above issues, we systematically investigated the effect of pressure on the IV–VI compounds. We chose PbX (X = Se, Te) and studied the evolution of their physical properties and crystal structure under pressure. Combining high-pressure electrical transport and synchrotron x-ray diffraction (XRD) measurements, we have drawn a phase diagram for PbSe and PbTe to reveal the internal correlation between the structural evolution and the electrical properties.

2.   Methods
  • Single crystals of PbSe were grown using a chemical vapor transport (CVT) method. High-purity Pb sheets (99.99%) and Se powder (99.99%) were mixed in the proportion of Pb: Se = 1:1 before loaded into a quartz ampoule. The chemical-loaded ampoule was gradually evacuated to vacuum of 10−5 torr and sealed. The sealed ampoule was laid in a two-zone horizontal furnace. The source zone and growth zone were heated to 1313 K and 1240 K, respectively, at a rate of 30 K/h. Then temperatures were kept for 5 h and slowly cooled down by 100 K in 10 h. At the completion of the run, the furnace was slowly cooled down to room temperature at a rate of 10 K/h. The as-synthesized single crystals were carefully collected after physical breaking of the ampule.

    Single crystals of PbTe were synthesized by mixing stoichiometric ratio of Pb sheets (99.99%) and Te powder (99.99%). The mixture was loaded into an alumina crucible and then stored in a quartz tube. Then the vacuum ampoule was slowly heated to 723 K in 12 h and heated to 1323 K in 7 h and kept for 6 h. Then the tube was steadily cooled to 1123 K in 6 h and subsequently air quenched to room temperature.

    Powder x-ray diffraction (XRD) was examined on a Bruker D2 powder x-ray diffractometer (Cu Kα radiation, λ = 1.54056 Å). Rietveld refinements of the powder XRD patterns were performed through the software of General Structure Analysis System (GSAS-II).[34] Scanning electron microscope (Phenom Pro) equipped with energy dispersive spectroscopy (EDS) was utilized to characterize the composition and detect the surface morphology of the single crystals. Electrical resistivity at ambient pressure was measured using a physical property measurement system (PPMS). We adopted a standard DC four-probe method with Au wires to obtain the electrical resistivity in a temperature range from 1.8 K to 300 K.

    A BeCu-type diamond anvil cell (DAC) with 200 μm culet was used to generate high pressure for transport measurements as described elsewhere.[35,36] A layer of cubic BN/epoxy composite was interposed between the BeCu gasket and the electrical contacts. Four pieces of Pt foils were positioned on the sample’s surface in accordance with the van der Pauw technique.[10,37,38] The high-pressure XRD experiments were conducted at the BL15U1 beamline of the Shanghai Synchrotron Radiation Facility, utilizing an x-ray wavelength of λ = 0.6199 Å. A piece of Re was used as the gasket and mineral oil was used as the pressure transmitting medium. The pressure was measured through the ruby luminescence method.[39] Rietveld refinements were applied with the GSAS-II to obtain the structural parameters.[34]

3.   Results
  • As shown in the insets of Figs. 1(a) and 1(b), both PbSe and PbTe samples show metallic luster. The synthesized PbSe and PbTe samples are characterized by the XRD and EDS measurements at ambient pressure. Figures 1(a) and 1(b) show the XRD patterns and Rietveld refinement results for PbSe and PbTe. All the peaks could be attributed to NaCl-type face-centered cubic (fcc) structure with space group of Fm3¯m. From the EDS data in Figs. 1(c) and 1(b), the chemical composition Pb: Se = 47.99:52.01 implies slight Pb vacancies in the as-grown samples, while Pb: Te = 53.94:46.06 with slight Te defects.

    Figure 2 displays the temperature dependence of the electrical resistivity ρ(T) of PbSe and PbTe ranging from 1.8 K to 300 K. Although electronic structure calculations indicate that both PbSe and PbTe compounds are narrow-gap semiconductors, the ρ(T) for both PbSe and PbTe reveal a metallic behavior in the normal state. We attribute such behavior to the self-doping due to deviations from stoichiometry, causing the variation of Fermi level to metal states. The insets of Fig. 2 show the resistivity in the low temperature region. The residual resistivity ratio [RRR = ρ (300 K)/ρ (1.8 K)] is 26.8 for PbSe and 60.3 for PbTe.

    Figure 3 shows the temperature dependence of the resistivity ρ(T) of PbSe under various pressures. In the low-pressure region, ρ(T) shows a metallic character similar to that observed at ambient pressure. Increasing pressure initially induces a continuous suppression of the overall magnitude of ρ. Subsequently, ρ(T) decreases rapidly with a minimum occurring at around 2.3 GPa and then increases abnormally. For P > 3.5 GPa, ρ(T) displays a semiconducting-like behavior, which is different from that observed in the low-pressure region. These unusual phenomena could be related to a pressure-induced topological phase transition manifested as the band-gap closure and following reopening.[40] Upon further compression, the resistivity reaches a maximum at a pressure above 7 GPa. At the same time, the curve displays a pronounced anomalous peak near 250 K, indicating the metal–insulator transition (TM–I). As the pressure is further increased above 7 GPa, ρ rapidly decreases. At 15.3 GPa, the normal state behaves as a metal. When the pressure increases to around 19.6 GPa, a small drop of ρ is observed below 6.5 K. When the pressure rises up to 23.7 GPa, the resistivity drop becomes more evident and zero resistivity is achieved at low temperature, indicating the emergence of superconductivity in PbSe under pressure.[33] Higher pressure suppresses the superconductivity as the Tc decreases. As shown in Fig. 3(e), the high-pressure experiments have been repeated on different samples with good reproducibility of the observed superconductivity transition temperatures. The occurrence of pressure-induced metallization and the following superconducting transition in PbSe are consistent with other MX semiconductors.[27,41–43]

    We also performed the electrical resistivity measurements of PbTe at various pressures from 1.8 K to 300 K. When the pressure is around 7.6 GPa, ρ(T) shows a metallic behavior as that at ambient pressure. The superconducting transition Tconset∼7.2 K is observed at 13.7 GPa and then decreases with pressure, revealing a negative pressure coefficient of Tc. In summary, a similar evolution of ρ (T) is observed for PbTe under high pressure, and this abnormal phenomenon is closely related to the structural phase transitions which will be discussed hereafter.

    The observed superconductivity in PbSe is further supported by the evolution of the resistivity–temperature curve with the magnetic fields applied as shown in Fig. 5(a). The superconductivity is suppressed with increasing magnetic fields. A magnetic field of about 4 T is adequate to suppress the superconducting transition under this pressure. The upper critical field μ0Hc2(T) is determined by ρ = 90%ρ0 (ρ0 is the initial resistivity before superconducting transition) on the resistivity–temperature curves, as shown in Fig. 5(b). Deviating from the Werthamer–Helfand–Hohenberg theory based on the single-band model,[44] the upper critical field μ0Hc2(T) of PbSe has a positive curvature. Similar behavior has been observed in MgB2, YNi2B2C, 2H-NbSe2 and isostructural superconductor PbS[41,45–49] but neither observed in Cr-doped PbSe nor In–I co-doped PbTe investigated before.[50,51] More detailed study is still required to confirm the multiband superconducting properties in PbSe under high pressure. A simple formula μ0Hc2(T) = μ0Hc2(0)[1 – (T/Tc)2]α/[1 + (T/Tc)2]β is used to fit the μ0Hc2(T) curves.[52] We obtain α = 1.50 and β = 2.02 for PbSe at 31.0 GPa, which is far from the value of 1 in the Ginzburg–Landau model.[53,54] The zero-temperature upper critical field is estimated to be 3.01 T at 31.0 GPa, which yields a coherence length ξ(0) of 10.3 nm according to the Ginzburg–Landau equation.[55] It is worth noting that the value of μ0Hc2(0) is well below the Pauli–Clogston limit. Similarly, the estimated μ0Hc2(0) is 3.65 T and 3.93 T at 24.6 GPa and 27.8 GPa, respectively. Figure 5(c) shows the evolution of the superconductivity of PbTe in the magnetic field at 23.7 GPa. The superconducting transition is gradually suppressed as the magnetic field increases to 2.4 T, with the extrapolated upper critical field μ0Hc2(0) to be 2.1 T (2.29 T) at 23.7 GPa (13.7 GPa), as shown in Fig. 5(d). The response of temperature dependence of the resistivity to magnetic fields in both PbSe and PbTe provides further evidence of the pressure-induced superconducting transition.

    To identify the origin of the superconducting transition and the anomaly in the resistivity curve, we chose PbSe to perform in situ high-pressure XRD measurements to analyze the structural evolution under various pressures. Figure 6(a) shows the high-pressure synchrotron XRD patterns measured at room temperature up to 72.6 GPa. As shown in the patterns below 4.6 GPa, we can index all the diffraction peaks of PbSe with the Fm3¯m phase. Beyond 5.9 GPa, we observe a structural transformation in particularly characterized by the emergence of a new diffraction peak near 2θ = 12.5°. The signal of Fm3¯m phase completely eliminates at around 9.0 GPa, which is consistent with the rapid decrease of resistivity in our electrical transport measurements in Fig. 3. Above 21.4 GPa, another phase transition takes place, as indicated by the new diffraction peaks in the XRD patterns in Fig. 6(a). Upon compression to 35.8 GPa, the XRD patterns remain the same shape and no further transitions are observed within 72.6 GPa. All the peaks can correspond to the phase with space group Pm3¯m.

    The representative fittings of the XRD patterns obtained at 3.4 GPa, 14.8 GPa, and 68.7 GPa are displayed in Fig. 6(b). Three phases with the space groups of Fm3¯m, Pnma and Pm3¯m are demonstrated by the reasonable refinements. The refinements yield model parameters of Rwp = 2.79% and χ2 = 2.44 for the Fm3¯m phase, Rwp = 4.26% and χ2 = 6.11 for the Pnma phase and Rwp = 1.77% and χ2 = 0.90 for the Pm3¯m phase. The corresponding fitting results are summarized in Table 1. Among the three phases, the Pnma structure can be created by an orthorhombic distortion from the Fm3¯m structure, and the atoms slide in Pnma could lead to the structure transition to Pm3¯m under higher pressure.[28,56]

    Figure 6(c) presents the pressure-dependent lattice parameters and volume of the three phases in PbSe. There are two coexistence regions around the phase transition pressures. The Fm3¯m phase coexists with Pnma phase between 5.9 GPa and 7.3 GPa, and Pnma phase is along with Pm3¯m phase between 27.5 GPa and 35.8 GPa. It should be noted that the Pnma phase has a doubled lattice period compared with the Fm3¯m phase. This phenomenon indicates that the phase transition from Fm3¯m to Pnma is mediated by a Peierls distortion.[28,56] The phase III is more symmetric in comparison with phase II, which suggests that phase III is derived by the pressure-suppressed Peierls distortion. In Fig. 6(b), we use a third-order Birch–Murnaghan equation of state to fit the volume–pressure relation. The equation is

    where B0 and V0 are the bulk modulus and unit-cell volume, respectively. The fitting yields B0 = 63.40 ± 5.13 GPa and V0 = 57.07 ± 0.33 Å3 for the Fm3¯m phase, B0 = 64.77 ± 3.4 GPa and V0 = 54.72 ± 0.44 Å3 for the Pnma phase and B0 = 227.36 ± 22.72 GPa and V0 = 43.68 ± 0.52 Å3 for the Pm3¯m phase. We use the volume per unit cell (Z = 4 for the Fm3¯m and Pm3¯m phases and Z = 1 for the Pnma phase) to elucidate the volume evolution of the three phases upon compression. The volume collapses from the Fm3¯m to Pnma phase and from the Pnma to Pm3¯m phase are 3.5% and 5.7%, respectively, providing the evidence of the first-order transition.

    Figure 7(a) shows the high-pressure phase diagram of PbSe encompassing the Tc, resistivity at typical temperatures and temperature coefficient of the resistivity (dρ/dT) acquired from transport measurements. These results demonstrate that high pressure dramatically alters both crystal and electronic structures of PbSe. Upon compression, PbSe experiences the similar evolution path as other IV–VI compounds: first from Fm3¯m structure to Pnma structure, and then to Pm3¯m structure. The resistivity of PbSe exhibits a nonmonotonic evolution with increasing pressure, which corresponds to a semiconductor–metal transition. In phase I, the resistivity is first suppressed with applied pressure and reaches a relatively low value at about 2.3 GPa. This peculiar behavior of resistivity is not associated with a structural phase transition because high-pressure XRD studies reveal structural stability in this pressure range. The emergence of the sharp valley has been identified as a signature of pressure-induced topological phase transition. A similar phenomenon was observed for black phosphorus,[57] Sb2Te3,[58] ZrTe2,[59] BiTeI,[60] and TlBiS2.[11] As the pressure further increases, the resistivity increases with a maximum occurring at around 7.0 GPa with a temperature-dependent metal–insulator transition, indicating the completion of the first structural transition.

    In phase II, the slope of the pressure dependent resistivity has an obvious change. The resistivity begins to decrease upon compression which is obviously different from the behavior in Cr-doped PbSe.[50] In phase III, the resistivity continuously decreases with pressure and exhibits typical metallic behavior. The slope becomes moderate under higher pressure. Superconductivity is observed in this pressure region and the Tc decreases monotonically with increasing pressure. The observed superconductivity in PbSe is associated with structural instability and/or pressure-induced structural phase transition. The suppression of superconductivity in phase III is probably due to a reduction of the density of state at the Fermi level as revealed by a study of PbS.[41]

    A quite similar evolution under high pressure is observed in PbTe. All the characteristic temperatures from our high-pressure experiments are summarized in a T–P phase diagram in Fig. 7(b). Pressure-induced non-monotonic evolution of resistivity and a metal–semiconductor transition occur in PbTe at the low-pressure region in accordance with the pressure of structural transition reported before.[23] Upon further compression, PbTe evolves into a metallic state at the normal state, and superconductivity is observed at low temperatures. The results presented above allow us to build the close relationship between the structural and physical properties for PbX material under high pressures. Further investigation combining first principles calculations could be significant to clarify the mechanism of the pressure-induced superconductivity in the IV–VI semiconductors.[41,61]

4.   Conclusion
  • In this work, we conducted a comprehensive characterization of the structural evolution and superconductivity of lead chalcogenides PbSe and PbTe. In situ high-pressure synchrotron XRD experiments along with Rietveld refinements confirmed the structural transition from the Fm3¯m to Pnma phase and then to the Pm3¯m phase. High-pressure electrical resistivity measurements demonstrated that both PbSe and PbTe exhibit a quite similar evolution under increasing pressure, from a semiconductor with higher resistivity to a metallic state. Superconductivity emerges when the material evolves into the high-pressure CsCl-type cubic phase. We built a phase diagram for PbSe and PbTe, which can also be extended to other similar IV–VI semiconductors.

Figure (7)  Table (1) Reference (61)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return