2025 Volume 34 Issue 2
Article Contents

Suixin Zhan, Shaokang Yuan, Yuming Bai, Fu Liu, Bohan Zhang, Weijia Han, Tao Wang, Shengxiang Wang, Cai Zhou. Thickness-dependent magnetic property of FeNi thin film grown on flexible graphene substrate[J]. Chinese Physics B, 2025, 34(2): 027503. doi: 10.1088/1674-1056/ad92fd
Citation: Suixin Zhan, Shaokang Yuan, Yuming Bai, Fu Liu, Bohan Zhang, Weijia Han, Tao Wang, Shengxiang Wang, Cai Zhou. Thickness-dependent magnetic property of FeNi thin film grown on flexible graphene substrate[J]. Chinese Physics B, 2025, 34(2): 027503. doi: 10.1088/1674-1056/ad92fd

Thickness-dependent magnetic property of FeNi thin film grown on flexible graphene substrate

  • Received Date: 16/08/2024
    Accepted Date: 09/10/2024
    Available Online: 01/01/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(5)

Article Metrics

Article views(188) PDF downloads(0) Cited by(0)

Access History

Thickness-dependent magnetic property of FeNi thin film grown on flexible graphene substrate

Abstract: Electronics over flexible substrates offer advantages of flexibility, portability and low cost, and promising applications in the areas of energy, information, defense science and medical service. In recent years, tremendous progress has been witnessed in the development of flexible wearable devices that can be potentially massively deployed. Of particular interest are intelligent wearable devices, such as sensors and storage cells, which can be integrated by flexible magnetoelectronic devices based on magnetic thin films. To examine this further, the magnetic properties of FeNi thin films with different thicknesses grown on flexible graphene substrate are investigated at room temperature. The coercivity increases with increasing thicknesses of FeNi thin film, which can be attributed to the increase of grain size and decrease of surface roughness. Moreover, the thickness modulated magnetic property shows a magnetic anisotropy shift increase with varying thicknesses of FeNi thin film by using measurements based on ferromagnetic resonance, which further enhances the resonance frequency. In addition, the resonance peak is quite stable after bending it for ten cycles. The result is promising for the future design of flexible magnetoelectronic devices.

1.   Introduction
  • Along with the rapid development and continual increase of information data in microwave technologies, soft magnetic materials used as imperative functional materials for information processing and storage have become an incredible cornerstone of modern information society.[1–3] Magnetic anisotropy,[4–6] one of the important intrinsic parameters for soft magnetic materials, determines the coercive field and magnetic moment orientation, which can influence the operating frequency and even power consumption. Thus, the investigations of mediation methods and the mechanism of magnetic anisotropy are essential issues in soft magnetic materials. Fan et al. have reported in-plane uniaxial magnetic anisotropy mediated by an oblique sputtering angle during sputtering in soft magnetic thin film grown on a Si substrate, which leads to an increase of resonant frequency.[7] We have investigated an electric-field control of magnetic anisotropy modulation in an epitaxial magnetic thin film on a Pb(Mg1/3Nb2/3)O3–30%PbTiO3 substrate.[8] Although the magnetic anisotropy of magnetic thin film can be modified by the methods of changing the oblique sputtering angle and the applied electric field, the point of rigid substrate inevitably impedes the flexible electronic device performances. Recently, flexible materials have been exploited to implement functionalities on flexible electronic devices, which exhibit more favorable properties than most of the rigid substrates in terms of weight saving, flexibility, mechanical reliability and excellent environmental toughness.[9–13] For example, Liu et al. have demonstrated a self-assembled periodic wrinkling surface structure in CoFeB thin films grown on polydimethylsiloxane membranes induced by applying uniaxial tensile strains to continuously tune high frequency magnetic properties.[14] Graphene film as another flexible substrate, compared with a polydimethylsiloxane substrate, has significant advantages, including high conductivity, mechanical strength, thermal stability, surface area, environmental friendliness, processability and biocompatibility.[15,16] He’s group has reported a flexible graphene film for radio-frequency antennas, multi-beam radiation, highly sensitive wearable sensors, etc.[17–19] In fact, graphene film as a flexible substrate is expected to spark a number of studies into flexible magnetoelectronic devices. In addition, FeNi thin film has received great attention due to its highly sought-after magnetic characteristics such as high saturation magnetization, which can be widely used in static and high-frequency for soft magnetic materials. Therefore, in this work, we report on the thickness-dependent magnetic property of FeNi thin film with different thicknesses grown on a flexible graphene substrate (FGS). With increasing thicknesses of the FeNi thin film, the grain continues to grow and the corresponding size becomes larger, which leads to the increase of coercivity. Meanwhile, the magnetic anisotropy — using measurements based on the ferromagnetic resonance (FMR) — increases, and the resonance peak is quite stable despite bending it for ten cycles. Moreover, different thicknesses of FeNi thin films grown on FGS realize an increase of resonance frequency from 3.8 GHz to 4.1 GHz and a decreasing trend of the permeability.

2.   Experiments
  • FeNi thin films with different thicknesses of 70 nm, 140 nm, 210 nm, and 280 nm, respectively, are deposited by radio frequency (RF) magnetron sputtering on the FGS at a common base pressure of 8 × 10−4 Pa and work processing Ar pressure of 1 Pa and a power of 50W, the thickness of the FGS is 100 μm. A field emission scanning electron microscope (SEM, Hitachi SU5000) is employed to observe the cross-section of the microstructures. The surface roughness is measured by an atomic force microscope (AFM) using an Asylum Research © MFP-3D. The x-ray diffraction (XRD) measurements are performed on an X’Pert x-ray powder diffractometer with Cu Kα radiation (1.54056 Å). The FMR measurements are carried out with a PNA 8722ES vector network analyzer using the coplanar waveguide method. Permeability spectra are carried out with a PNA E8363B vector network analyzer using the microstrip method. An upright metallurgical microscope (Soptop RX50M) is employed to observe the surface morphology microstructures.

3.   Results and discussion
  • In the FeNi/FGS structure, the in-plane magnetic hysteresis loop of the sample with a thickness of 70 nm is shown in Fig. 1(a). It exhibits a weak in-plane magnetic uniaxial anisotropy, which can be attributed to the oblique sputtering. The slight oblique columnar structure is observed by a SEM cross-section image (see the inset in Fig. 1(a)), which indicates the good quality of FeNi thin film grown on the FGS. Similar results can also be obtained in samples with FeNi film thicknesses of 140 nm, 210 nm and 280 nm. The saturate magnetic field Hs and coercivity Hc are extracted from these magnetic hysteresis loops, as shown in Fig. 1(c). With increasing thicknesses of FeNi thin film, Hs and Hc increase from 370 Oe to 1210 Oe and from 46 Oe to 78 Oe, respectively, as shown in Fig. 1(b), which may be caused by the increase of grain size. This can be proved by XRD results in the following section.

    Figure 2(a) presents the crystal structures of FeNi/FGS samples. The sharp diffraction peak (004) of the FGS is located at 54.5°. The (111) peak of FeNi thin film appears at 44.2°, which indicates the polycrystalline feature of FeNi thin film grown on the FGS. The intensity of the (111) peak increases with the increasing thickness of the FeNi thin film, which implies an enhancement of the crystallization. Moreover, the width of the peaks decreases as thicknesses increase, revealing the increase of the grain size. According to the Scherrer equation, grain sizes of FeNi thin films are indeed denoted as increasing from 8.3 nm to 11.9 nm with increasing thickness of FeNi thin films from 70 nm to 280 nm, which is consistent with the result of Hc obtained from VSM measurement. In addition, the surface roughness values, measured by the AFM, decrease from 15 nm to 7 nm, as shown in Fig. 2(b). By increasing the thickness of the FeNi thin film, the grain size increases, as shown in Fig. 2(a), which indicates that less grain boundary will be produced. This result can lower the magnetic moment’s scattering in the FeNi thin film and make the magnetic moment align in one direction easier, further leading to the increase of the coercivity of FeNi thin film. Generally, the less the grain boundary, the more the microstructural defects are reduced.[20] Moreover, internal stresses usually develop around the grain boundary. Considering the decrease of the grain boundary with the increasing thickness of the FeNi thin film, the total internal stress might decrease.[21] It can be beneficial to keep the magnetization direction of the magnetic moment, which leads to the large magnetization reversal magnetic field. According to the above results and the random anisotropy model,[22] this result can influence the dynamic magnetic properties of the FeNi thin film grown on FGS, which will be discussed in detail below.

    Generally, magnetic thin film applications are based on analyses of dynamic magnetic or magnetization processes. Moreover, the effect of magnetic interactions is much more salient in high-frequency magnetization dynamics due to the nonlinear effect, particularly at magnetic resonance frequencies. In order to investigate the thickness-dependent magnetic anisotropy for these samples of FeNi/FGS, the dynamic magnetic property is measured by FMR using a vector network analyzer with a coplanar waveguide method. Figure 3(a) shows the schematic illustration of FMR. For 210 nm-thick FeNi thin film, the typical FMR spectra are obtained as shown in Fig. 3(b) (solid dots). In general, the magnetization is probed by using a special phase correlation under the microwave excitation; the FMR spectrum does not correspond to the imaginary part of the susceptibility alone, but in fact represents a mixture of the imaginary and real parts. Therefore, the actual function of the absorption curve can be fitted by an asymmetric Lorentzian function[23]

    where H is the external magnetic field, Hr is the magnetic resonance field, ΔH is the half-width at half-maximum of the linewidth, θ is the phase that mixes the real and imaginary parts of the dynamic susceptibility, and A is the integral coefficient. Figure 3(b) shows the result of fitting of the FMR curves using Eq. (1) (silver lines). The resonant magnetic field increases from 467 Oe to 1957 Oe as the micro frequency increases from 6 GHz to 12 GHz for 210 nm-thick FeNi thin film. Similar results can be obtained for all thin films. As a result, figure 3(c) shows the data of frequency-dependent Hr under different thicknesses of FeNi thin film (solid dots), which is fitted by using Kittel’s equation[24]

    where the gyromagnetic ratio γ/2π = 2.8 GHz/kOe, 4πMeff is the effective magnetization, and Hk is the in-plane magnetic uniaxial anisotropy field. Figure 3(d) shows the corresponding fitting curves (silver lines). Meanwhile, the values of 4πMeff and Hk can be extracted by fitting frequency-dependent Hr curves using Eq. (2). 4πMeff appears to remain almost constant as the thickness of FeNi thin film increases from 70 nm to 280 nm. However, Hk obviously increases from 103 Oe to 186 Oe with increasing thicknesses of FeNi thin films. These results can be explained by the increase of the FeNi grain size with increasing thicknesses of FeNi thin films. This result can lead to the increase of resonance frequency.

    The dependence of permeability on the frequency with different thicknesses of FeNi thin films is measured by a vector network analyzer with the microstrip method. Figures 4(a) and 4(b) show the dynamic real part μ′ and imaginary part μ″ of the complex permeability spectra of FeNi thin film measured at 200 Oe magnetic field ranging from 1 GHz to 9 GHz. The real part μ′ exhibits a dispersive-type curve, while a Lorentzian shape resonance curve is shown for imaginary part μ″, which reveals a typical resonance permeability spectrum. The permeability μi decreases with increasing thicknesses of FeNi thin films, as shown in Fig. 4(c). However, the imaginary permeability spectra of FeNi thin film with increasing thicknesses from 70 nm to 280 nm display clear resonance frequency peaks, increasing from 3.8 GHz to 4.1 GHz (Fig. 4(d)). These results are consistent with the results of Hk-dependent thickness of FeNi thin films, and further confirm that the thickness of FeNi thin film grown on FGS can mediate the magnetic property. In flexible magnetoelectronic apparatus, the permeability of magnetic thin film can directly determine the performance and sensitivity of magnetic devices. In magnetic devices such as antennas and sensors, magnetic thin film is used to detect subtle changes in the magnetic field. The high permeability of magnetic thin film can lessen the hysteresis loss and eddy current loss, further helping to improve the sensitivity and resolution of magnetic devices. This result can strengthen the accuracy of the detection of magnetic field intensity for sensors and enhance signal transmission efficiency for antennas. In this work, with decreasing thicknesses of FeNi thin film, a high permeability is obtained, which can satisfy the need for high sensitivity of magnetic devices. However, high resonance frequency can only be gained by increasing the thickness of the FeNi thin film; this is a persistent requirement for the increase of work frequency in communication equipment. In fact, the preferred approach to the higher resonance frequency and/or higher permeability is dependent on the application scene.

    To verify the performance of the FeNi thin film after mechanical bending, the sample of FeNi (210 nm)/FGS is placed on a customized automatic counting slide rail, and tested after different bending cycles, as shown in Fig. 5. The FMR curves begin to deform after bending for ten cycles, whereas cracks can be observed and an obvious resonance peak is obtained. With increasing bending to twenty cycles, more cracks can be seen, while the resonance peaks disappear. Cracks in metal films appeared inside large grains and between small grains,[25] which can influence the grain size and magnetic resonance property. The cracks may lead to the disappearance of the resonance field’s peak in FeNi thin film in this work. The above results are obtained under a bending speed of 1 s per cycle. When the bending speed increases to 10 s per cycle, a similar result can be observed.

4.   Conclusion
  • In summary, we have identified the microstructure and dynamic magnetic property of FeNi thin film with different thicknesses grown on FGS. With increasing thicknesses of FeNi thin film, the magnetic anisotropy is demonstrated to increase by measurement of the FMR. This result can be attributed to the crystal structure of FeNi thin film with different thicknesses. Moreover, the resonance peak is quite stable after bending for ten cycles. In addition, a clear resonance peak of FeNi thin film changing from 3.8 GHz to 4.1 GHz and a decrease of permeability are obtained. These results remove the obstacles of transmission distance and the signal quality of communication systems.