2025 Volume 34 Issue 2
Article Contents

Ziyu Li, Tianyi Gu, Wenqi Wei, Yang Yuan, Zhuo Wang, Kangjian Luo, Yupeng Pan, Jianfeng Xie, Shaozhe Zhang, Tao Peng, Lin Liu, Qi Chen, Xiaotao Han, Yongkang Luo, Liang Li. Elastic properties of Cu–6wt% Ag alloy wires for pulsed magnets investigated by ultrasonic techniques[J]. Chinese Physics B, 2025, 34(2): 020701. doi: 10.1088/1674-1056/ada1c8
Citation: Ziyu Li, Tianyi Gu, Wenqi Wei, Yang Yuan, Zhuo Wang, Kangjian Luo, Yupeng Pan, Jianfeng Xie, Shaozhe Zhang, Tao Peng, Lin Liu, Qi Chen, Xiaotao Han, Yongkang Luo, Liang Li. Elastic properties of Cu–6wt% Ag alloy wires for pulsed magnets investigated by ultrasonic techniques[J]. Chinese Physics B, 2025, 34(2): 020701. doi: 10.1088/1674-1056/ada1c8

Elastic properties of Cu–6wt% Ag alloy wires for pulsed magnets investigated by ultrasonic techniques

  • Received Date: 09/11/2024
    Accepted Date: 18/12/2024
    Available Online: 01/01/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(4)  /  Tables(1)

Article Metrics

Article views(172) PDF downloads(1) Cited by(0)

Access History

Elastic properties of Cu–6wt% Ag alloy wires for pulsed magnets investigated by ultrasonic techniques

Abstract: Conductor materials with good mechanical performance as well as high electrical and thermal conductivities are particularly important to break through the current bottle-neck limit (∼100 T) of pulsed magnets. Here, we perform systematic studies on the elastic properties of the Cu–6wt% Ag alloy wire, which is a promising candidate material for the new-generation pulsed magnets, by employing two independent ultrasonic techniques, i.e., resonant ultrasound spectroscopy (RUS) and ultrasound pulse-echo experiments. Our RUS measurements manifest that the elastic properties of the Cu–6wt% Ag alloy wires can be improved by an electroplastic drawing procedure as compared with the conventional cold drawing. We also take this opportunity to test the availability of our newly-built ultrasound pulse-echo facility at the Wuhan National High Magnetic Field Center (WHMFC, China), and the results suggest that the elastic performance of the electroplastically-drawn Cu–6wt% Ag alloy wire remains excellent without anomalous softening under extreme conditions, e.g., in ultra-high magnetic field up to 50 T and nitrogen or helium cryogenic liquids.

1.   Introduction
  • High magnetic fields play an important role in modern material science and condensed matter physics. On the one hand, the magnetic field is one of the key control parameters, and many intriguing phenomena can be induced by high magnetic field, such as integer or fractional quantum Hall effect,[1–3] quantum magnetization plateau,[4] quantum critical point,[5] Fulde–Ferrell–Larkin–Ovchinnikov (FFLO) state,[6,7] re-entrance of superconductivity,[8] etc. On the other hand, a high magnetic field also acts as a “magnifier” to physical ensembles, e.g., by reducing the magnetic length lB≡ħ/(eB), quantum oscillations are amplified, and thus Fermi surface topology of materials can be more resolvable;[9] by enhancing the ratio B/T, the thermal fluctuations will be suppressed so that phenomena related to quantum fluctuations can be more observable; by promoting the signal-to-noise ratio (S/N ∝ B3/2), the resolution of nuclear magnetic resonance can be greatly increased;[10,11] etc. In this sense, pulsed field, currently the only non-destructive method to create magnetic field higher than 46 T, has attracted great interest in the past decades. However, due to multiple factors, including electrical conductivity, thermal conductivity, strength of conducting wires, electromagnetic coil winding technique, and others, so far the amplitude of pulsed field has been limited to ∼100.75 T (which is the world record that was set by Los Alamos National Laboratory, USA).[12]

    One of the central issues in the development of ultra-high pulsed-field magnets is to manufacture proper conducting wires with excellent mechanical performance. Cu–Nb macro-composite and Cu–Ag alloy are the two materials that are commonly used for the inner coil of pulsed magnets. For instance, in the 1990s, Japan successfully created a high magnetic field exceeding 80 T by Cu–Ag alloy;[13] more recently, Wuhan National High Magnetic Field Center (WHMFC) in China has created a magnetic field of ∼94.8 T by using Cu–Nb conductors.[14,15] Compared with Cu–Nb macro-composite, the conductivity of Cu–Ag alloys is generally higher, which is beneficial to reducing Joule heating; and moreover, to reach a similar strength, the draw ratio η required is relatively smaller.[13] For Cu–Ag alloy, the mechanical and electrical properties depend strongly on the fabrication methods. For example, Sakai et al. reported ultra-high strength and high conductivity in Cu–Ag cold drawing combined with intermediate heat treatment.[16–18] In particular, the optimized Cu–24wt% Ag wire with η = 5.8 shows ultimate tensile strength (UTS) of 1.5 GPa and an electrical conductivity of 65% IACS (International Annealed Copper Standard) at room temperature.[13] For Cu–6wt% Ag with lower expense, the electrical conductivity can be enhanced to 80% IACS; nevertheless, the UTS is much lower.[19] This trade-off relation between strength and electrical conductivity of Cu–Ag alloys restricts their scope of application.[20] Recently, Chen et al. successfully manufactured the Cu–6wt% Ag alloy wire of rectangular section 3 mm × 5 mm via electrically-assisted drawing. It was found that by an electroplastic drawing (ED) process, the UTS, elongation and electrical conductivity of Cu–6wt% Ag alloy wire can be enhanced by 8%, 4%, and 30%, respectively,[21,22] strongly suggesting the potential application for the 110 T project at WHMFC.

    However, we noticed that although the fabrication method and the resultant UTS of Cu–Ag alloys have been well studied, little is known about their elastic properties, especially at liquid-nitrogen temperature where these conducting wires typically work for pulsed magnets. In addition, we are also curious about their performance under ultra-high field, which, in principle, should have been a prerequisite for their use as conductor materials in pulsed magnets, but was omitted previously. In this paper, by a combination of resonant ultrasound spectroscopy (RUS) and ultrasound pulse-echo experiments, we report the elastic properties of Cu–6wt% Ag alloy wires at both atmosphere and extreme conditions. The main results are summarized in Table 1. Our results show that the elastic properties of Cu–6wt% Ag alloy wires can be improved by an ED procedure, and the performance remains excellent without anomalous softening under ultra-high magnetic field up to 50 T and low temperature down to 1.9 K.

2.   Experimental details
  • Oxide-free copper and silver with a purity of 99.99% (Cu–6wt% Ag) were selected and melted in an argon atmosphere. A Cu–Ag alloy ingot of 120 mm in length and 90 mm in diameter was then prepared by the conventional cast method. The ingot was heated at 780 °C for 2 hours and quenched in water for solid solution treatment. Subsequently, the ingot was forged to a diameter of approximately 70 mm and underwent heat treatment at 450 °C for 20 hours, followed by cooling to room temperature in the furnace. The aged ingot was hot forged to 40 mm in diameter. Finally, a rod with a diameter of 12 mm was produced by rotary forging and drawn into a rectangular conductor wire of 3 mm × 5 mm. Drawing reduction was given in teams of logarithmic strain by draw ratio η≡ln(A0/A), where A0 and A represent the initial and final cross-sectional areas, respectively. When the draw ratio reached η = 5.1, a part of the alloy was drawn by electrically assisted drawing (sample ED), while the other part was drawn by conventional cold drawing (sample CD). The deformation process is described in Fig. 1(a). In this work, the electrically assisted drawing processing instrument was used by adding a pulse power supply to a conventional wire-drawing machine. A pulse square-wave electric source was self-made to provide a high-density current during the drawing. Electrically assisted drawing applies current to the deformation area of the metal wire. Current density of 50 A/mm2, duration time of 10 ms, and duty ratio of 50% were applied in the experiment. Under the condition of a drawing speed of 5 m/min, a tungsten steel alloy drawing die was used. In order to compare the effect of drawing process on the mechanical properties of the material, both samples were taken when the draw ratio η = 6. More details about the sample preparation can be found in Refs. [21,22].

    Elastic properties of Cu–6wt% Ag alloy wires were investigated by two different ultrasonic related techniques: RUS and ultrasound pulse echo. For RUS measurements, the Cu–6wt% Ag samples were polished into parallelepipeds, and the dimensions were 0.957 mm × 1.243 mm × 1.319 mm (ED) and 0.916 mm × 1.219 mm × 1.349 mm (CD). RUS measurements were carried out in a lock-in technique by sweeping frequency from 0.3 MHz to 3 MHz at stabilized temperatures ranging from 5.4 K to 300 K in a helium-flow cryostat (OptistatCF, Oxford). A schematic of the RUS apparatus is presented in Fig. 1(b). The sample is corner-touch installed between two LiNbO3 transducers with the bottom one acting as ultrasound transmitter (TX) and the top one as receiver (RX). When the frequency of the excitation approaches a characteristic vibrational mode of the sample, a resonant peak will be picked up in RX. Alumina hemispheres were used between LiNbO3 and sample, for insulation and mechanical protection.[23] For more details about RUS technique, we refer to Refs. [24,25].

    For ultrasound pulse-echo measurements, the elastic constants were determined by measuring the ultrasound velocity in the principle of time-of-flight.[26] The Cu–6wt% Ag samples were polished into parallelepipeds with dimensions 5.164 mm × 3.929 mm × 3.024 mm (ED) and 5.972 mm × 5.030 mm × 2.733 mm (CD). A pair of Y10-cut LiNbO3-type transducers with fundamental vibration frequencies 30 MHz (longitudinal) and 18 MHz (transverse) were glued on the two parallel faces of each sample. The longitudinal ultrasound velocity vL with k∥u (where k is the ultrasound propagation vector, and u is displacement vector) was measured by using a home-built integrated dual-mode pulse-echo ultrasonic measurement system at WHMFC.[27] The measurement of transverse ultrasound velocity was also tried, but no detectable signal was observed for unknown reasons. The elastic constant C11 was calculated via C11=ρvL2, where ρ = 8.732 g/cm3 is the mass density. These measurements were carried out under extreme conditions, with temperatures down to 1.9 K and magnetic fields up to 50 T.

3.   Results and discussion
  • Figures 2(a) and 2(b), respectively, show representative vibrational spectra of Cu–6wt% Ag alloy wire samples, taken at room temperature. A series of resonant peaks can be recognized. According to the principle of RUS technique, one can compute all the resonant frequencies with provided elastic constants {Cij} (i,j = 1,…,6), sample dimensions, and density.[24,28,29] Conversely, with a series of known resonant frequencies, density, and sample dimensions, we can also derive {Cij} by a mathematical fitting process. The fitting continues until the root mean square (RMS) ≡{∑i[(fcali−fexpi)/fexpi]2}/N minimizes, where N is the number of identified resonant peaks, and fexpi and fcali are frequencies of the ith experimental (black bars in Fig. 2) and calculated (red bars) resonance modes, respectively. For isotropic polycrystalline samples, there are only two independent elements in the {Cij} tensor, viz C11 and C44, and all the elastic moduli can be calculated as follows:[24] shear modulus

    bulk modulus

    Young’s modulus

    and Poisson’s ratio

    At room temperature, the derived elastic constants for the ED and CD samples of Cu–6wt% Ag are summarized in Table 1. We notice that all elastic constants C11, K, E, and G are slightly larger in the ED sample, while their Poisson’s ratios are comparable. Acoustic Debye temperature ΘD and lattice thermal conductivity κL at 300 K (T≳ΘD) are also calculated according to the elastic constants.[30–32] Both ΘD and κL are larger in the ED sample, as expected. However, since the total thermal conductivity should also include the contribution from electrons, it is premature to draw a precise conclusion before direct thermal conductivity measurements are made.

    The elastic properties of Cu–6wt% Ag samples at low temperature were also studied by RUS. Figure 3(a) presents the spectra of the Cu–6wt% Ag ED sample at selected temperatures between 5.4–300 K. One clearly finds that all the resonant peaks move to higher frequency upon cooling, implying that the material hardens at low temperature. The same trend is also seen in the CD sample (data not shown). The extracted temperature dependent elastic constants are displayed in Figs. 3(b)–3(f). We find C11, bulk modulus K, shear modulus G, and Young’s modulus E all increase as temperature decreases, while below ∼50 K these elastic constants tend to level off; the overall temperature dependencies can be well described by an empirical Varshni’s expression c(T) = c0–s/(eT*/T–1), where c = Cij, K, G, or E,[33] as denoted by the red lines. Another prominent feature is that all through the temperature range 5.4–300 K, all these elastic constants are larger in the ED sample. In particular, at the liquid nitrogen temperature where Cu–6wt% Ag alloy wires are used as current carrier of pulsed magnets, the ED treatment can enhance the moduli C11, K, G, and E by 2.7(1)%, 4.3(1)%, 0.3(1)%, and 0.7(1)%, respectively. Poisson’s ratio ν is another physical quantity that should be discussed here. ν measures the extent of expansion of a material in directions perpendicular to the specific direction of compressing. At 300 K, ν = 0.348 for both samples. As is well known, ν sits in the range 0.25–0.35 for most conventional metals;[34] this is the case for both ED and CD Cu–6wt% Ag alloys. However, the temperature dependent ν of the two samples behave differently: while ν of the CD sample is almost constant, data of the ED sample increase slightly at low temperature. Therefore, on the whole, ν is a little larger in the ED sample. Since ν characterizes the ductility, the relatively larger ν in ED implies more ease in coil winding, which is also advantageous for pulsed magnet application.[31]

    The elastic constants measured from RUS can be verified by an alternative ultrasound technique, the pulse-echo measurement. The principle of ultrasound pulse-echo is sketched in Fig. 1(c). To start with, a representative result for the ED sample at 300 K is displayed in Fig. 4(a). After a single excitation of longitudinal ultrasound pulse (k∥u), a series of echoes are clearly identified, whose amplitudes decay following an exponential law and can be well fitted to u(t) = Aexp(−βvt)+u0, where A is a prefactor, and u0 is a constant. The fitting yields β = 1.35(5) cm−1, which in turn gives rise to the ultrasound attenuation coefficient αL = 11.7(4) dB/cm. The position of each echo is plotted versus n in the inset to Fig. 4, the slope of which leads to the average time interval between echoes, τ = 2.2159(4) μs. The longitudinal ultrasound velocity can thus be calculated, vL = 4660.8(9) × 103 m/s. With these, C11 = 189.69(7) GPa can be deduced. This result is in close agreement with that determined by RUS, cf. Table 1. The CD sample was also measured by ultrasound pulse echo experiment, and C11 = 185.12(8) GPa was obtained. It is important to mention that both RUS and pulse echo measurements reveal enhanced C11 in the ED sample, implying that the ED procedure does improve the elastic performance of Cu–6wt% Ag alloy wire, albeit that such an improvement is weak. A natural question, then, concerns why the ED procedure can lift the UTS substantially, but only enhances the elastic properties relatively weakly? In order to clarify this issue, more investigations based on micro-structure experiments and systematic stress-strain measurements will be needed in the future.[22]

    To explore the performance of the ED sample under extreme conditions, we also investigated its elastic properties by ultrasound pulse echo measurements at low temperature down to 1.9 K and high magnetic field up to 50 T. By the so-called quadrature procedure and the phase-shift analysis,[35] the relative change in the ultrasound velocity ΔvL/vL is measured as a function of magnetic field at fixed temperatures. For example, ΔvL/vL at 78 K is shown in Fig. 4(b); furthermore, the converted C11 is presented in Fig. 4(c). Irrespective of the relatively large noise, a slight increase of C11 with B is visible, for both 78 K and 1.9 K, while no drastic softening can be seen up to 50 T. Note that for pulsed magnet application, the Cu–Ag alloy wires are used when immersed in liquid nitrogen. In this sense, our results thus demonstrate that Cu–6wt% Ag ED exhibits a good elastic performance for this purpose. Here, we must admit that the measurement precision under pulsed field is much lower than that in the absence of field, likely due to the sample vibration caused by pulsed field and/or eddy-current heating effect. Technically, how to reduce the noise level will be a special concern for us in the future.

4.   Conclusion
  • In conclusion, by a combination of RUS and ultrasound pulse-echo experiments, we systematically studied the elastic properties of Cu–6wt% Ag alloy wires. Our results show that an ED procedure can improve the elastic performance of Cu–6wt% Ag alloy wires, and the elastic performance remains excellent under extreme conditions, e.g., in ultra-high magnetic field and nitrogen or helium cryogenic liquids.

Figure (4)  Table (1) Reference (35)