2025 Volume 34 Issue 4
Article Contents

Wen Chen, Min Li, Bao-Qin Fu, Tun Chen, Jie-Chao Cui, Qing Hou. Effect of copper/tungsten heterophase interface on radiation resistance: Insights from atomistic simulations[J]. Chinese Physics B, 2025, 34(4): 046108. doi: 10.1088/1674-1056/adb40d
Citation: Wen Chen, Min Li, Bao-Qin Fu, Tun Chen, Jie-Chao Cui, Qing Hou. Effect of copper/tungsten heterophase interface on radiation resistance: Insights from atomistic simulations[J]. Chinese Physics B, 2025, 34(4): 046108. doi: 10.1088/1674-1056/adb40d

Effect of copper/tungsten heterophase interface on radiation resistance: Insights from atomistic simulations

  • Received Date: 14/10/2024
    Accepted Date: 09/12/2024
    Available Online: 01/04/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(8)  /  Tables(1)

Article Metrics

Article views(359) PDF downloads(1) Cited by(0)

Access History

Effect of copper/tungsten heterophase interface on radiation resistance: Insights from atomistic simulations

Abstract: Nanostructured materials have demonstrated superior radiation-damage tolerance compared to their coarse-grained counterparts, contributing to the extended lifespan of nuclear materials. However, the mechanisms underlying this enhanced irradiation resistance remain unclear. In this study, we present atomistic simulations to investigate the impact of Cu/W heterophase interface on the evolution of irradiation-induced defects. The simulation results reveal that the Cu/W interfaces can act as defect sinks, effectively trapping self-interstitial atoms (SIAs). Furthermore, the interface demonstrates both the interstitial emission and interstitial transfer mechanisms, wherein the trapped W SIAs facilitate the emission of Cu atoms from the interface to the Cu side. These emitted Cu SIAs can promote defect recombination on the Cu side, leading to a reduced defect concentration in the Cu/W nanomultilayers. Consequently, these combined mechanisms contribute to a lower overall concentration of irradiation-induced defect, thereby enhancing the radiation resistance of Cu/W nano-multilayers.

1.   Introduction
  • Materials employed in nuclear reactors are subjected to high-fluence and high-energy neutron irradiation.[1–3] This results in the generation of a substantial number of Frenkel pairs (FPs), i.e. self-interstitial atoms (SIAs) and vacancies.[4,5] Defect accumulation can lead to the degradation of materials’ properties. Nanostructured materials[6–12] have garnered considerable interest due to their superior radiation-damage tolerance compared to their coarse-grained counterparts,[13] contributing to the extended lifespan of nuclear materials. This enhanced tolerance is attributed to their extremely high dense grain boundaries (GBs),[6,13] and heterophase interfaces,[14] which effectively absorb and annihilate radiation-induced defects. Such characteristics reduce the concentration of radiation-induced defects, improve swelling resistance, and maintain the morphological stability of multilayered microstructures.[7–10,15] Especially, they preferentially absorb SIAs over vacancies, significantly influencing the radiation resistance of nuclear materials.[16,17]

    Besides directly absorbing defects, Bai et al.[6] observed that GBs in pure copper (Cu) can re-emit trapped SIAs, allowing them to recombine with nearby vacancies through the interstitial emission (IE) mechanism. Li et al.[17] reported on the segregation and annihilation processes of vacancies and SIAs near the GBs. Additionally, Liu et al.[14] found that the Cu/niobium (Nb) heterophase interface preferentially traps Cu SIAs rather than Nb SIA, which is subsequently released to recombine with Cu vacancies on the Cu side. These findings highlight the complex interaction between defects and GBs/heterophase interfaces, which plays a crucial role in enhancing radiation-damage tolerance.

    Owing to its high thermal conductivity, Cu has emerged as a potential heat sink material for future nuclear fusion reactors.[18] Tungsten (W) is considered a promising plasma-facing material for these reactors because of its exceptional properties, including high melting point, excellent thermal conductivity, and low sputtering yield.[19] Cu/W nano-multilayers[12,15,20] have been proposed as candidate structures for connecting W and Cu in diverters. The crystal structures of Cu and W are distinct; Cu exhibits a face-centered cubic (FCC) configuration, while W adopts a body-centered cubic (BCC) configuration. Theoretically, an incoherent FCC–BCC heterophase interface between Cu and W serves as an effective defect sink,[8,12] significantly influencing the evolution and recovery of radiation-induced defects. Recent experimental studies[9,10,15] on Cu/W nano-multilayers subjected to He ion irradiation have demonstrated remarkable radiation-damage tolerance. These studies indicate that the Cu/W nano-multilayers with smaller period-thickness exhibit stronger radiation resistance, as evidenced by less pronounced changes in interface texture[10] and a lower concentration of vacancy-type defects.[9] However, detailed insights into how heterophase interfaces influence the evolution of irradiation-induced defects and enhance the radiation resistance of Cu/W nano-multilayers remain lacking.

    This study aims to address these gaps through molecular dynamics (MD) simulations of Cu/W nano-multilayers. These nano-multilayers possess a polycrystalline structure, with W(110) and Cu(111) serving as the primary diffraction planes.[8,21,22] The Kurdjumov–Sachs[23] (KS) orientation relation at the Cu(111)/W(110) heterophase interface forms the basis for the atomic model used in the simulations. This study investigates the effects of Cu/W heterophase interfaces on the evolution of SIAs and explores the underlying mechanisms that enhance the radiation resistance of Cu/W nano-multilayers.

2.   Model and methods
  • This study utilizes the graphics processing unit (GPU)-accelerated Molecular Dynamics Package of Sichuan University (MDPSCU)[24] to conduct MD simulations. The embedded atom method (EAM) interatomic potential developed by Zhou et al.[25] is employed for simulating the Cu–W systems. This potential has demonstrated its reliability in various atomic simulation studies.[12,21,26]

    Figure 1 displays the prepared Cu/W nano-multilayers simulation box. Previous researches[11,21] have shown that the mismatch between two metals affects their interaction. Thus, simulations require a minimal mismatch for accuracy and representation. Thus, in this study, the Cu/W simulation box is constructed by joining the Cu with the W simulation boxes, ensuring a mismatch of less than 0.058%. Periodic boundary conditions are applied in all three directions. Table 1 lists the computed parameters for the simulation box.

    The lattice length a0Cu of Cu is initially set to be 3.615 Å. For convenience, the lattice length of W (3.165 Å) is expressed as 0.87552a0Cu. Considering the lattice mismatch between Cu and W, as well as the undetermined distance between Cu and W interfaces in the Cu/W model,[11,21] we adjust a0Cu from 3.603 Å to 3.627 Å (12 data points) to identify the stable state of the Cu/W model. Cu/W nano-multilayers can serve as joining materials for plasma-facing materials (W) and heat sink materials (Cu) with operating temperatures ranging from 450 K to 1050 K.[27–29] Therefore, the simulation system is then thermalized to 700 K by assigning the atomic velocities according to the Maxwell distribution. Subsequently, the system is subjected to an NVT ensemble, simulating for approximately 500 ps at 700 K to achieve stable interface structures, before being quenched to 0 K. We employ the gradient descent method to minimize the system’s energy and calculate the potential energy versus lattice length curve. Using the least squares method, we fit the data points with a cubic polynomial to model this curve. Subsequently, Newton’s optimization method is applied to determine the minimum energy point on the fitted curve, yielding a corresponding a0Cu value 3.61446 Å. This approach ensures that the simulation box could attain its most stable or ground state after thermodynamic relaxation.

  • To explore the underlying mechanisms by which Cu/W heterophase interfaces enhance radiation resistance, we initially examine the evolution of the Cu/W heterophase interface as it continuously traps Cu or W SIAs. Specifically, the Cu (W) SIAs are inserted into the system containing Cu/W interface in an accumulative pattern. The SIAs are randomly positioned within the first three Cu monolayers (for Cu SIAs) and two W monolayers (for W SIAs) along the interface. In this region, the interface exhibits a strong absorption for SIAs (Fig. 6(a)). After each insertion, the system is firstly quenched to 0 K, then thermalized to 700 K, and subsequently allowed to evolve freely for approximately 40 ps. This duration is sufficient for the SIA to be absorbed by the interface. In total, 160 Cu (W) SIAs are inserted into the system.

    To further compare the influence of Cu and W SIAs on Cu/W interface, 160 Cu SIAs and 160 W SIAs are introduced simultaneously into one system. During each introduction step, one Cu SIA and one W SIA are inserted together. The Cu SIAs are still placed within the first three Cu monolayers along the interface, while the W SIAs are positioned within the first two W monolayers. Other simulation details remain the same as previously described. The structural evolution of the nano-multilayer system after quenching to 0 K was tracked using common neighbor analysis (CNA).[30] implemented in OVITO.[31]

    We also calculate the formation energies of single SIAs at various locations to explore their interactions with the interface. This analysis involves uniformly and randomly introducing a single Cu (W) SIA into the Cu (W) side of the Cu/W model. To reduce statistical errors, a total of 1700 independent simulation boxes are used (800 boxes for single Cu SIAs and 900 boxes for single W SIAs). After the introduction, the systems are quenched to 0 K, and the distribution of the SIAs is subsequently analyzed. The interstitial formation energy Ef is given by[12]

    where ESIA–int is the total energy of the Cu/W system containing a defect induced by the insertion of a single Cu or W SIA, Ecoh represents the cohesive energy of a Cu or W atom in the bulk, and Eint is the total energy of the Cu/W system without defects.

3.   Simulation results
  • Considering the roles of GBs in pure Cu[6,32] and W,[33] the Cu/W heterophase interface[9,10,34] may also exhibit a distinct IE mechanism[6,14] for mitigating radiation damage. To explore this possibility, we investigate the evolution of the interface after trapping Cu SIAs, W SIAs, and a mixture of both. Figure 2 illustrates the evolution of the interface as it continuously absorbs Cu SIAs. As shown in Figs. 2(a)–2(c), Cu SIAs trapped by the interface remain on the Cu side. As more Cu SIAs are trapped, the interfacial Cu plane becomes disordered, leading to an increase in non-FCC Cu atoms that grow towards the Cu side along the interfacial Cu plane (Figs. 2(d)–2(i)). Conversely, there is no significant alteration in the atomic configurations on the W side. These results indicate that the IE mechanism indeed plays a role when the interface traps Cu SIAs.

    However, the situation is different when the interface traps W SIAs. The evolution of the interface as it continuously absorbs W SIAs is presented in Fig. 3. Unlike the observations in Figs. 2(a)–2(c), where Cu SIAs are introduced, the insertion of W SIAs on the W side does not lead to any obvious alteration in the structure and atomic configurations of the W side (Figs. 3(a)–3(f)). On the contrary, W SIAs trapped by the interface migrate from the W side to the Cu side, as shown in Figs. 3(a)–3(c). These trapped W SIAs adopt a BCC configuration, displacing Cu atoms from their original positions, which facilitates the emission of Cu atoms from the interface to the Cu side. As more W SIAs are trapped, the number of non-FCC atoms increases, growing towards the Cu side along the interfacial Cu plane (Figs. 3(d)–3(f)). This behavior contrasts with the IE mechanism reported in Refs. [6,14,17]. Instead, the Cu/W heterophase interface exhibits an interstitial transfer (IT) mechanism, where interface-trapped W SIAs can facilitate the emission of Cu atoms from the interface to the Cu side.

    It seems that inserting 160 W SIAs on the W side causes more severe damage to the adjacent Cu layer than inserting the same number of Cu SIAs on the Cu side, as shown in Figs. 2 and 3. To further compare the influence of Cu and W SIAs on Cu/W interface, Cu SIAs and W SIAs are introduced simultaneously into a single simulation box. Figure 4 presents the results. All Cu SIAs remain on the Cu side, while the W SIAs continue to migrate from the W side to the Cu side, similar to the result shown in Fig. 3. Consequently, compared to the results from the previous two simulations (Figs. 2 and 3), significant structure deformation also occurs on the Cu side and more non-FCC atoms appear. This phenomenon indicates that the IT and IE mechanisms can work synergistically when the interface simultaneously traps W SIAs and Cu SIAs. The predominant deformation on the Cu side is consistent with observations made when the Cu/W heterophase interface is subjected to tensile loading.[26,35] This behavior can be attributed to Cu’s relatively lower mechanical strength compared to W, leading to the presence of Cu/W interface greatly weakening the deformability of Cu.[26]

    Figure 5 displays the atomic configurations of the Cu (Figs. 5(a)–5(c)) and W (Figs. 5(d)–5(f)) layers along the interface when the interface simultaneously traps W SIAs and Cu SIAs. As shown in Figs. 5(a) and 5(d), the initial atomic structures of the interface exhibit a regular arrangement pattern, similar to phenomena reported in Refs. [12,22,36]. This regular pattern is associated with the in-plane array of misfit dislocation nucleates, which serve as geometrically favorable sites for dislocation emission.[26,36–39] As shown in Figs. 5(a)–5(c), the increasing number of trapped Cu and W SIAs disrupts this regular arrangement pattern. Non-FCC atoms and Shockley partial dislocations proliferate along the interfacial Cu plane and extend toward the Cu side. In contrast, although BCC W atoms also proliferate along the interfacial W plane, the W plane remains flat (Figs. 5(d)–5(f)). These observations are consistent with the findings in Figs. 2–4. As trapped SIAs cause a transformation from the regular arrangement pattern to a distorted pattern in the interface structure, the emission locations of Shockley partial dislocations and the growth of non-FCC atoms become decoupled from the initial atomic structures of the interface. This differs from the findings reported in Refs. [26,36].

  • The W SIA-loaded Cu/W heterophase interface triggers the IT mechanism, rather than the more commonly recognized IE mechanism. Therefore, gaining further insight into this IT mechanism is essential. We investigate the interactions between single SIAs and the interface. As noted in Subsection 2.2, all independent simulation boxes are ultimately quenched to 0 K. The final positions of defects induced by the inserted SIAs are determined using Wigner–Seitz (WS) defect analysis.[40] The identified defects include Cu SIAs, W SIAs, and combined Cu–W combinations. A Cu–W combination contains a BCC W and a Cu SIAs. Thus, it reflects the growth of BCC W toward the Cu side. Figure 6 illustrates the distribution of these defects. As indicated by the region enclosed by red dashed lines in Fig. 6(a), after inserting Cu SIAs, the defect concentration within the first atomic layer on the Cu side is considerably higher than that in the second to fourth atomic layers near the interface. Conversely, no defects are observed within the first atomic layer on the W side when inserting W SIAs; instead, some migrate to the Cu side (green spheres). The green spheres in Fig. 6(b) represent two types of W atoms, which help explain the phenomenon observed in Fig. 6(a). The first type consists of W atoms that have combined with neighboring Cu atoms, forming Cu–W combinations. The second type includes W atoms that facilitate the emission of Cu SIAs. Thus, even single W atoms trapped by the interface (green spheres) could promote Cu emission from the interface to the Cu side (cyan spheres), albeit with a very low probability. This finding is consistent with the results shown in Figs. 2–4. Therefore, while substantial absorption occurs when all SIAs migrate near the interface, the interface’s influence on Cu SIAs extends further than that on W SIAs.

    Based on the quenched simulation boxes, we calculate the average interstitial formation energy Ef of defects induced by inserted Cu SIAs (Fig. 7(a)) and W SIAs (Fig. 7(b)). The results show that the Ef of individual Cu and W SIAs within the bulk are approximately 3.15 eV and 9.72 eV, respectively. Notably, the Ef for a single Cu SIA significantly decreases to 1.47 eV (Fig. 7(a)) near the interface. In contrast, a single W SIA cannot exist near the interface. Using WS defect analysis and visualization tools implemented in OVITO, we observe that when inserting W SIAs, the defects in the first layer on the Cu side, indicated by the green square in Fig. 7(b), are Cu–W combinations with Ef = 2.06 eV. Additionally, single Cu SIAs emitted as a result of W SIA insertion are identified in the second to third atomic layers away from the interface (in the region enclosed by cyan lines), with formation energies of 3.46 eV and 3.7 eV, respectively. This phenomenon can be attributed to the absorption of single W atoms by the interface, which leads to the emission of a single Cu SIA toward the Cu side (denoted by the left insert of Fig. 7(b)), consistent with the observations in Fig. 6(b).

    We further investigate how a single trapped W SIA facilitates the emission of a Cu SIA to the Cu side and the recombination of Cu SIA with vacancy. As shown in Figs. 8(a) and 8(b), when a single W SIA migrates close to the interface and becomes trapped, it directly displaces Cu atoms along its migration path, leading to the emission of a Cu SIA toward the Cu side. Subsequently, the emitted Cu SIA moves toward the Cu vacancy at the third atomic layer near the interface and recombines with it (Figs. 8(c) and 8(d)).

4.   Discussion
  • Radiation damage in Cu/W single crystal leads to the generation of numerous FPs, specifically SIAs and vacancies. SIAs can immediately recombine with nearby vacancies upon thermal activation.[41,42] In contrast, Cu SIAs and W SIAs that are further away from vacancies migrate freely.[41] These mobile SIAs not only recombine with other vacancies but also cluster with additional SIA-type defects, forming larger SIA clusters, such as dislocation loops. Additionally, they migrate to surfaces, contributing to the formation of new layers.[43–45] Meanwhile, vacancies migrate and aggregate, leading to the formation of vacancy clusters, such as voids.[32,42,43] The continuous microstructural changes due to radiation damage contribute to material deterioration, significantly shortening the lifespan of nuclear materials.

    Here, we explore how Cu/W nano-multilayers influence the evolution of irradiation-induced defects, focusing on the critical role of SIA migration. In Cu/W nano-multilayers, both Cu and W SIAs can be trapped by Cu/W heterophase interfaces. Once trapped, these atoms tend to accumulate on the interfacial Cu plane, resulting in the growth of non-FCC atoms, predominantly on the Cu side (Figs. 2 and 3). The SIA-loaded Cu/W heterophase interface demonstrates two distinct mechanisms: the IE mechanism and the IT mechanism. In the IT mechanism, the trapped W SIAs can facilitate the emission of Cu atoms from the interface to the Cu side, even in the absence of Cu vacancies near the interface and Cu SIAs at the interface (Fig. 3). This behavior contrasts with that observed at the Cu/Nb heterophase interface, where Cu SIAs[14] are preferentially trapped and subsequently released to the Cu side, rather than Nb SIAs. Both the IE and IT mechanisms promote the emission of Cu SIAs from the interface and facilitate recombination with vacancies on the Cu side.

    Therefore, multiple mechanisms enhance the radiation resistance of Cu/W nano-multilayers. First, the interface absorbs defects, especially SIAs, resulting in reduced irradiation-induced defects within the bulk. Second, the interfaces favor the recombination of defects on the Cu side through the IE and IT mechanisms. Consequently, the overall irradiation-induced defect concentration is lowered.

5.   Conclusions
  • Atomistic simulations are conducted to investigate the influence of Cu/W heterophase interface on the evolution of irradiation-induced defects. The simulation results reveal that the interface serve as a defect sink, effectively trapping SIAs. The SIA-loaded interface demonstrated two mechanisms for inducing the emission of Cu atoms from the interface to the Cu side: the IE mechanism and the IT mechanism. The IE mechanism occurs when the interface traps Cu SIAs, while the IT mechanism, plays a role when the interface traps W SIAs. Both mechanisms facilitate defect recombination, contributing to the enhanced radiation resistance of Cu/W nano-multilayers.

Figure (8)  Table (1) Reference (45)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return