2025 Volume 34 Issue 5
Article Contents

Rui-Qiang Song, Chuang Liu, Yi-Yang Long, Ji-Feng Han, Jing Ren, Sen Qian. A high light-yield neutron scintillator based on Ce3+-doped lithium glass[J]. Chinese Physics B, 2025, 34(5): 050703. doi: 10.1088/1674-1056/adb94b
Citation: Rui-Qiang Song, Chuang Liu, Yi-Yang Long, Ji-Feng Han, Jing Ren, Sen Qian. A high light-yield neutron scintillator based on Ce3+-doped lithium glass[J]. Chinese Physics B, 2025, 34(5): 050703. doi: 10.1088/1674-1056/adb94b

A high light-yield neutron scintillator based on Ce3+-doped lithium glass

  • Received Date: 30/12/2024
    Accepted Date: 13/02/2025
    Available Online: 01/05/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(7)  /  Tables(1)

Article Metrics

Article views(1164) PDF downloads(9) Cited by(0)

Access History

A high light-yield neutron scintillator based on Ce3+-doped lithium glass

Abstract: The development of low-cost and highly efficient thermal neutron detection materials to substitute the rare and expensive 3He gas is important for applications requiring thermal neutron detection. Lithium-based glass (Li glass) is a promising candidate due to its simple fabrication process and low cost. This paper reports the optical properties and scintillation performance of a new Ce3+-doped Li glass, whose luminescence efficiency is significantly enhanced with a light yield of about 4770 ph/MeV, which is about 54% of that of BGO crystal, and the energy resolution is 14.5% for 662 keV gamma rays. The Ce3+-doped Li glass shows a high light yield of about 7058 ph/neutron, which is about 1.18 times that of the reference GS20 glass. The Ce3+-doped Li glass exhibits stronger gamma ray suppression capability compared to GS20 glass samples. Further optimizing the Ce3+ concentration and 6Li content is expected to achieve much superior neutron detection efficiency, positioning it as a promising alternative to 3He gas for efficient thermal neutron detection.

1.   Introduction
  • Thermal neutron detectors play an important role in applications such as nuclear safety, medicine, industrial neutron imaging and resource exploration. With the establishment of large scientific facilities and the development of nuclear science and technology,[1,2] the demand for thermal neutron detection is increasing. The shortage of 3He gas has accelerated the development of high-performance alternative materials for neutron detection.[3] Doping certain neutron-sensitive nuclides into solid scintillation materials is an effective method for neutron detection, where high-energy secondary charged ions are generated upon neutron capture, and numerous optical photons are further generated in the scintillator through ionization of these secondary ions, which can be changed to electric signal through photon-electric devices.[4–7] The desired properties for scintillators used in neutron detection include high light yield, short decay time, non-hygroscopic nature, large neutron capture cross-section and good neutron/γ discrimination capability. In practice, 6Li and 10B are commonly incorporated into solid scintillators to achieve higher thermal neutron capture efficiency. Therefore, many scintillators containing 6Li and 10B have attracted extensive attention, including boron-containing plastic scintillators,[8] boron-containing glass scintillators,[9] lithium-containing crystal scintillators,[10] lithium-containing glass scintillators[11] and lithium-containing plastic scintillators.[12] Comparing boron and lithium-containing scintillators, 10B(n, α)7Li reaction has a higher thermal neutron capture cross-section (∼ 3840 barns) than that of 6Li(n, t)4He reaction (∼ 940 barns).[13,14] Although the thermal neutron reaction cross-section of 10B is higher than that of 6Li, the reaction Q-value of 10B(n, α)7Li is about 2.31 MeV, which is lower than the value of 4.78 MeV for 6Li(n, t)4He.[15] Therefore, lithium-containing scintillators can generate much larger neutron signals and are more suitable for thermal neutron detection. The plastic scintillators mainly consist of low-atomic-number (Zeff) nuclides, such as H and C, which are very efficient for high-energy neutron detection through elastic scattering, but the energy resolution is not good. There is a method to add 10B to the plastic to make it sensitive to thermal neutrons, but the quenching effect is very heavy, and a neutron and gamma discrimination method is needed.[16]

    There are many lithium-containing crystal scintillators, especially inorganic scintillators such as ZnS/LiF,[17] LiI:Eu2+,[18] LiBaF3:Ce,[19] Cs2LiYCl6:Ce[20] and Cs2LiLaBr6:Ce.[21] These crystal scintillators have better transparency, higher detection efficiency and better resolution. In addition, multi-mode detection of neutrons and gamma rays by pulse shape discrimination (PSD) is possible.[22,23] However, crystal scintillators are susceptible to moisture, making them difficult to use in extreme environments.[24] Crystals are typically grown using the Czochralski method, micro-pulling-down method, or the Bridgman method.[25,26] These growth processes are rigorous, costly, and it is difficult to process single-crystal scintillators to large sizes. Lithium-containing glass scintillators (Li glass) are inert and have high transparency, which ensures excellent stability and light output efficiency. Compared to crystal scintillators, glass is easy to process into any shape and size due to the non-salting nature of the melting process, offering significant advantages in large-size preparation and fiber optics preparation for radiation monitoring in various environments. Furthermore, glass is easily moldable, allowing continuous adjustment of the composition to facilitate the development of suitable scintillators. Currently, 6Li-glass scintillators are widely used in thermal neutron detection and spectroscopy.[27,28]

    The optical and scintillation properties of scintillation materials are predominantly governed by the selection of luminescent centers and substrates. Rare earth elements have garnered significant research interest owing to their exceptional chemical stability and outstanding luminescent properties. The rare earth element luminescent center of the 4f–5f transition exhibits enhanced stability in fluorescence performance, with a narrower emission band that remains impervious to external influences. Furthermore, the 4f–5d transition enables the generation of a wide range of fluorescence emissions, from ultraviolet to near-infrared light.[29] The ions commonly used as luminescent centers in glass scintillators are Ce3+ and Eu2+. Compared to Eu2+ ions, the decay time of the Ce3+ emission center is on the order of ns, while that of Eu2+ is ∼ μs.[30] The luminescence generated by Ce3+ as the luminescent center of the glass scintillator has higher light output, good energy resolution, faster decay time, and is currently the best activator in scintillating glass.[31] In addition, the efficient halides can provide an ideal low-phonon-energy halide environment for the activator, which maintains the benefits of high transparency of oxide glass while improving chemical durability and thermal stability.[32] However, due to the amorphous nature of glasses, carriers tend to be trapped by many defect sites in the amorphous matrix, resulting in relatively low light yield (< 1000 ph/MeV) and poor optical properties for most glasses. Therefore, only a small number of commercially available lithium glasses exhibit high light yield, e.g., Ce3+ doped lithium alumino-silicate glass (GS20), with a gamma light yield of ∼ 4000 ph/MeV and a neutron light yield of ∼ 6000 ph/MeV, are primarily used for thermal neutron detection.[33,34]

    With the rapid development of neutron detection technology, neutron detection materials face increasingly stringent requirements in terms of detection efficiency, energy resolution and neutron/γ discrimination. It has been reported that oxide glasses offer excellent stability, while fluoride crystals have the advantage of low phonon energy.[35] Sr2GdF7:Tb3+ glass-ceramics combine the advantages of oxide glasses and fluoride crystals to exhibit strong optical properties and high light output, with XEL-measured intensities up to 194% of that of BGO.[35] This research study has made significant progress in improving the light output of glass scintillators. To improve the light yield of glass scintillators, we have combined the advantages of oxides and fluorides to study the Li glass performance at high Ce3+ content. The incorporation of 6Li in the glass matrix increases the sensitivity to thermal neutrons. This study aims to develop low-cost Li glass with high light yield, which is expected to be used in large-area neutron detection and neutron imaging.

2.   Experimental equipment and methods
  • The high Ce3+-doped Li glass in this study was synthesized using a conventional high-temperature melt-quenching technique. High-purity (4N) raw materials from Aladdin Co. were precisely weighed according to the target glass composition. The starting materials were homogenized using a planetary ball mill (with ZrO2 grinding balls), dried and sieved for subsequent use. Prior to melting, the mixed powder was loaded into an alumina crucible and pre-calcined in a muffle furnace at 800 °C. The pre-calcined product was then reground in the planetary ball mill to ensure homogeneity. The homogenized powder was transferred back into the alumina crucible and melted in a tube furnace at 1400 °C under a continuous gas flow (H2 and N2 mixture) to reduce oxygen, which is used to facilitate the reduction of Ce4+ to Ce3+. The molten glass was rapidly quenched into a preheated stainless-steel mold at 500 °C. The solidified glass was immediately transferred to an annealing furnace, where it underwent stress-relief treatment for several hours before cooling down. Finally, the annealed glasses were subsequently cut into specimens and polished to optical-grade surface quality for optical transmission, luminescence, and scintillation performance evaluations. The Ce3+-doped glass was cut into cubes of 5 × 5 × 5 mm3 size, and 25 × 25 × 5 mm3 size, as shown in Fig. 1. The Ce3+-doped Li glass shows enough transparency to see the pattern on the backside. The Ce3+-doped Li glass shows intense blue light under UV excitation, as shown in Fig. 1(b).

    A UV spectrophotometer and a spectrograph were utilized for spectroscopy measurements. The scintillator was enclosed on five sides with Teflon film, while silicon grease served as the optical coupling agent. The study employed a Hamamatsu S13360-6025CS Silicon Photomultiplier (SiPM), which has an effective area of 6 × 6 mm2 and a pixel size of 25 μm. It was operated using the Hamamatsu C12332-01 driver circuit. For detector calibration, gamma-ray spectra were measured using a 137Cs gamma-ray source. To evaluate the neutron response of the Ce3+-doped Li glass, an Am–Be neutron source with an activity of 0.51 MBq was used. Signals from the SiPM were recorded using a high-speed digitizer (DT5751), and the data were subsequently transmitted to a computer via a high-speed communication line for storage. A comparative test was conducted using commercial BGO and GS20 glass scintillators under identical testing conditions to evaluate the performance of the novel Ce3+-doped Li glass in gamma and neutron detection.

3.   Measurements with Ce3+-doped Li glass
  • Transmittance spectra of the Ce3+-doped Li glass are shown in Fig. 2. This glass has a high transmittance exceeding 80% in the range of 390–800 nm. The optical transmission performance in the blue and near-infrared wavelength bands is good, enabling coupling with photon-electric devices.

    The normalized photoluminescence (PL) and photoluminescence excitation (PLE) spectra of the high Ce3+-doped Li glass, are shown in Fig. 3. The PL spectrum shows that the glass scintillator has a broadband emission in the range of 360–600 nm. The emission peak at about 400 nm under the 354 nm excitation peak is mainly attributed to the transition in the 5d–4f bands of Ce3+ ions.[36] A Stokes shift of 47 nm of the PL and PLE spectra indicates a relatively weak self-absorption in the glass, which facilitates the transport of scintillation light.

    The light yield of scintillators is converted by the photon detection efficiencies (PDE) of SiPM and the XEL emission spectrum of the scintillator.[37] The x-ray excitation emission (XEL) spectra of the Ce3+-doped Li glass and a commercial BGO standard sample with the same size of 5 × 5 × 5 mm3 are shown in Fig. 4. The Ce3+-doped Li glass exhibits broad emission in the range of 350–500 nm under x-ray excitation. The emission peak is located at about 390 nm, and the XEL spectrum of Ce3+-doped Li glass is very similar to that of GS20 glass.[11] The emission peak of the BGO scintillator is located at about 470 nm. It is important to select a photodetector that can be adapted to the glass scintillator for light collection. The spectral response of SiPM is from 270–900 nm and the peak-sensitive wavelength is 450 nm. The photon detection efficiency curve (data from the Hamamatsu product brochure) is shown as a red dotted line in Fig. 4. The formula for calculating the light yield is as follows:[37]

    where ME is the channel number of the full-energy peaks, S is the single photoelectron channel number, εPDE is the weighted photon detection efficiency (PDE) of the SiPM and E is the energy of the γ-ray source. The unit of light yield is photons per MeV, indicating the number of photons that can be produced when 1 MeV gamma-ray is absorbed by the scintillator.

  • The commercial GS20 standard sample and BGO crystal were used to compare the light yield of Ce3+-doped Li glass. These three scintillators were coupled to the same SiPM for measurements with a 137Cs gamma-ray source. The gamma-ray spectra of Ce3+-doped Li glass, GS20 glass and BGO crystal are shown in Fig. 5. The full energy peak of the high-Ce3+-doped Li glass is not prominent when compared to the Compton plateau due to the low density (2.47 g/cm3) and small size, but the complete full peaks can be observed. The channel numbers were obtained by Gaussian fitting of the full-energy peaks for 137Cs at 662 keV. By fitting the full energy peaks, the energy resolution (ΔE/E) of BGO crystals is about 10.0%, while that of Ce3+-doped Li glass is about 14.5%. The channel numbers of the full-energy peak for the Ce3+-doped Li glass and the BGO crystal are 35430 and 68670, respectively. Therefore, the light yield of the BGO crystal is about 8843 ph/MeV, and the light yield of the Ce3+-doped Li glass is about 4770 ph/MeV. The light yield of the Ce3+-doped Li glass is equivalent to about 54% of the BGO crystal.

    Due to the low density (2.5 g/cm3) and small thickness (only 1 mm) of the GS20 glass sample, the full-energy peak is unclear. By Gaussian fitting of the full-energy peak on a logarithmic scale, the energy resolution is about 26.0%, with the center channel number of the full-energy peak at 20853. Therefore, the light yield of the GS20 glass sample is about 2807 ph/MeV. The measured light yield of the GS20 glass sample was smaller than the reported value of 4000 ph/MeV,[34] possibly because the thickness is too small and there are drawbacks inside the tested sample. The light yield of the Ce3+-doped Li glass is equivalent to about 170% of the tested GS20 glass sample and about 119% of the reported GS20 glass. The measurement uncertainty of the light yield mainly comes from the accuracy of the instrument as well as the measurement. After several measurements, the uncertainty of the light yield is found to be around 5%.

  • Since 6Li has a high thermal neutron capture cross-section (∼ 960 barns), the Ce3+-doped Li glass has good thermal neutron detection capability. The neutron response of the Ce3+-doped Li glass and GS20 glass sample were compared under an Am–Be neutron source. Neutrons were moderated to thermal neutrons by an 8 cm thick layer of paraffin in front of the Am–Be source with an activity of 0.51 MBq. To shield the high-energy gamma rays generated by the Am–Be neutron source, a 5 cm thick lead brick was placed behind the moderator. A fast PMT (XP2020 PMT) is used to measure the decay time of the Ce3+-doped Li glass. The neutron-averaged waveform was obtained by 800 pulses, as shown in Fig. 6.

    The decay curves were fitted with a double exponential function. The fitting function is expressed as

    Based on Eq. (2), the scintillation decay time is divided into two main components; a fast component and a slow component. The fast component decay time is about 58 ns (57.86%) and the slow component decay time is about 415 ns (42.14%).

    The neutron spectra of the Ce3+-doped Li glass and GS20 glass sample under the Am–Be neutron source are shown in Fig. 7. Two peaks corresponding to thermal neutrons are clearly observed. The Gaussian fitting of the thermal neutron peaks of the Ce3+-doped Li glass and the GS20 glass sample indicated channel numbers 79200 and 54040, respectively. The relative width (FWHM/mean) of the thermal neutron peak for the Ce3+-doped Li glass is about 10.5%, which is better than the 24.0% of the GS20 sample. It is worth noting that natural lithium with 6Li enrichment of 7.5% is used in this work, which means the neutron detection efficiency will be greatly enhanced if 95% enriched 6Li is used as that of the GS20 glass sample.

    The neutron light yield of Ce3+-doped Li glass is about 7058 ph/neutron, and the neutron light yield of the GS20 glass sample is about 4816 ph/neutron. The measured light yield of the GS20 glass sample was smaller than the reported value of 6000 ph/neutron.[34] The neutron light yield of Ce3+-doped Li glass is equivalent to about 147% of the tested GS20 glass sample and about 118% of the reported GS20 glass. In addition, the gamma light yield of the Ce3+-doped Li glass is 4770 ph/MeV, which is higher than that of 4000 ph/MeV for the GS20 glass sample.[33]

    In the glass matrix, high-energy gamma rays or charged particles induce ionization within the scintillator material. The energy of the liberated electrons is transferred to activator ions (e.g., Ce3+), which will excite their valence electrons to higher energy states. Subsequent radiative transitions of these electrons back to the ground state result in photon emission at characteristic wavelengths. For the Ce3+-doped Li glass, the excitation can migrate to Ce3+ ions and render recombination of the Ce3+ ions, resulting in further light emission. Thus, enhancing energy transfer from electron–hole excitation to Ce3+ ions is the key issue to increasing light yield. From the perspective of neutron capture, a higher content of 6Li is preferred to increase the neutron reaction possibility. However, an excessive content of Li+ will increase the difficulty of converting Ce4+ ions to Ce3+ ions, and a high content of Li+ will render the existence of non-bridging oxygen energy trapping centers.[38,39] Therefore, the concentration of Li and Ce in the glass matrix must be carefully balanced during melting. A ‘H2/N2’ mixed gas is used to create a low oxygen environment to ensure that most of the scintillating ions in the glass matrix exist as Ce3+. In addition, Al2O3 is added to the Li glass melting process to reduce the concentration of non-bridging oxygen and decrease the melting temperature, which is beneficial for shaping the Li glass. After melting and shaping, the glass is transferred to an annealing furnace to eliminate internal stress. Using the above mentioned methods, the light yield of Ce3+-doped Li glass can be effectively improved.

    When the neutrons are captured by the scintillator, the 6Li(n, t)α reaction produces high-energy α and tritium particles. These high-energy particles interact with atoms or molecules in the scintillator to produce quenching effects, resulting in varying degrees of energy loss from the particles.[40] The quenching factor (q) represents the ratio of the detected energy relative to the deposited energy, the larger q indicates a smaller energy loss of the incident particle. The q is defined as[41]

    where Eeq. is the measured equivalent electron-volt energy, EN is the incident neutron energy and Q is the Q-value of the reaction. The EN is negligible for thermal neutrons and the Q-value is 4.78 MeV. The neutron energy spectra were calibrated by gamma equivalent energy to obtain the neutron energy corresponding to the thermal neutron peaks. For Ce3+-doped Li glass and the GS20 glass sample, the Eeq. was calculated to be 1.48 MeV and 1.71 MeV, respectively. The resulting quenching factors of the Ce3+-doped Li glass and the GS20 sample are 0.31 and 0.36, respectively, for the 6Li(n, t)α reaction. The quenching factor (q) of the Ce3+-doped Li glass is slightly lower than that of the GS20 glass sample.

    For the Ce3+-doped Li glass and the GS20 glass sample, the pulse shapes of neutrons and gamma rays are similar, making it difficult to discriminate using the pulse shape discrimination method. However, conventional pulse height analysis or pulse integration methods are used because the neutron signals are similar and much larger, forming a neutron peak on the high-energy side, while the gamma rays are mainly distributed on the low energy side due to the low density of the Li glass. The ratio of gamma rays that are located within the neutron peak can be used to represent the neutron/γ discrimination performance. The gamma-ray spectrum can be deduced by fitting the energy spectrum without the neutron peak, and the components of gamma rays within the neutron peak can be calculated. Therefore, by fitting the spectrum of the neutron peak and the gamma ray background, the quantitative evaluation of the gamma-ray suppression capabilities of Ce3+-doped Li glass and the GS20 glass sample is acquired. Comparing the neutron energy spectra of the two glass scintillators reveals differences in the proportion of gamma rays at the neutron peaks, which can lead to an increased misclassification rate for neutrons. By performing Gaussian fitting of the thermal neutron peaks and employing a quadratic polynomial to deduce the gamma ray background, the percentage of gamma rays within the range of three times the standard deviation (sigma) is obtained. For the thermal neutron peak, the percentage of gamma rays in Ce3+-doped Li glass is approximately 13.8%, while in the GS20 glass sample the percentage of gamma rays is approximately 24.1%. The Ce3+-doped Li glass has a lower misclassification rate for neutrons than the GS20 glass sample, indicating better neutron/γ discrimination performance.

    As shown in Table 1, the physical and scintillation characteristics of Ce3+-doped Li glass were compared with those of commercial GS20 glass and other types of Li glass. The scintillation decay times of the Ce3+-doped Li glass were measured as 58 ns (fast component) and 415 ns (slow component). The fast component originates from the radiative recombination of Ce3+ ions acting as activators in the scintillator. Specifically, the 5d → 4f de-excitation transition of Ce3+ dominates the fast decay process.[43] This is attributed to the electric dipole-allowed nature of the 4f → 5d excitation transition in Ce3+, which typically exhibits broadband emission and a short decay time.[44] In contrast, the slow component is likely associated with spontaneous emission processes involving transitions from higher-energy excited states to the final ground state.[45] Compared to the GS20 glass samples, Ce3+-doped Li glass exhibits longer light attenuation components, likely attributed to the higher Ce3+ concentration. In addition, the Ce3+-doped Li glass and the GS20 glass scintillator have low densities, which can effectively reduce sensitivity to γ-rays, benefiting neutron detection and achieving good neutron and gamma discrimination. Furthermore, the Ce3+-doped Li glass exhibits a higher light yield for both gamma and neutron when compared to the GS20 glass sample. Therefore, it can be expected that the Ce3+-doped Li glass can be a viable substitute for the GS20 glass scintillator, offering a potential alternative to 3He gas.

4.   Conclusion
  • In summary, the high Ce3+-doped Li glasses were prepared using the high-temperature melting method, and the photoluminescence and scintillation properties were evaluated. Under UV and x-ray irradiation, emission peaks were observed at about 400 nm and 390 nm, which is due to the 5d–4f transition of Ce3+ ions. The pulse integration spectrum under 137Cs γ-ray radiation exhibited a high light yield of 4770 ph/MeV and an energy resolution of 14.5%@662 keV. In addition, the neutron light yield of the Ce3+-doped Li glass is about 7058 ph/neutron and the relative width of the thermal neutron peak is about 10.5% under Am–Be neutron source irradiation. The neutron yield of the Ce3+-doped Li glass was found to be about 1.18 times that of commercial GS20 glass, and the number of gamma rays that might be wrongly identified as neutrons is about 13.8%. This is much better than the value of 24.1% for the GS20 glass sample, which indicates much better neutron/γ identification performance was achieved. The quenching factor (q) of the Ce3+-doped Li glass is 0.31 for the neutron reaction, which is slightly lower than the 0.36 for the GS20 glass sample. In the future, the structure of the glass material and the relationship between structure and luminescence will be studied in detail. The formulation and process will continue to be optimized to improve the quenching factor of Li glass and further increase the content of 6Li to improve the neutron detection efficiency. The high Ce3+-doped Li glass will be a low-cost and high-efficiency neutron scintillator, which is favorable for applications in large-area neutron imaging detectors.

Figure (7)  Table (1) Reference (45)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return