Mengyuan Tang, Chuhan Tang, Sheng-Yi Xie, Fuxiang Li. Molecular dynamics simulations of ferroelectricity in P(VDF-TrFE)[J]. Chinese Physics B, 2025, 34(6): 067701. doi: 10.1088/1674-1056/adbbc1
Citation: Mengyuan Tang, Chuhan Tang, Sheng-Yi Xie, Fuxiang Li. Molecular dynamics simulations of ferroelectricity in P(VDF-TrFE)[J]. Chinese Physics B, 2025, 34(6): 067701. doi: 10.1088/1674-1056/adbbc1

Molecular dynamics simulations of ferroelectricity in P(VDF-TrFE)

  • Received Date: 11/01/2025
    Accepted Date: 25/02/2025
    Available Online: 01/06/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(6)  /  Tables(1)

Article Metrics

Article views(825) PDF downloads(4) Cited by(0)

Access History

Molecular dynamics simulations of ferroelectricity in P(VDF-TrFE)

Abstract: Poly(vinylidene fluoride-trifluoroethylene) (P(VDF-TrFE)) is a derivative of polyvinylidene fluoride (PVDF), known for its excellent ferroelectric properties, optical characteristics, chemical stability, and flexibility, making it a promising material for applications in electronic devices. In this study, the polarization switching mechanism of the β-phase of P(VDF-TrFE) is investigated using the polarized crystal charge method, along with molecular dynamics simulations. The simulation results show that the saturation polarization value is approximately 5.3 μC/cm2, and a coercive field of around 0.5 V/nm is required to switch its polarization states. By fitting the polarization reversal curve with the Kolmogorov–Avrami–Ishibashi model, it is observed that the data in the asymptotic and switching regions closely align with the predictions of the model, and the Avrami index n consistently ranges between 1 and 2. The polarization reversal is completed within approximately 10 ps, demonstrating high-speed dynamic behavior. Additionally, we predict that the ferroelectric phase transition occurs between 420 K and 430 K, with stable polarization performance maintained over a wide temperature range, which is consistent with experimental results.

1.   Introduction
  • The study of ferroelectric materials spans several decades, with the concept of ferroelectricity first proposed by French scientists in 1920.[1] Ferroelectric materials exhibit spontaneous polarization at certain temperatures, and the direction of this polarization can be reversed under the influence of an applied electric field. These materials have gained significant attention due to their excellent dielectric, piezoelectric, pyroelectric, photoelectric, and nonlinear optical properties.[2–5] However, research on ferroelectrics has predominantly focused on inorganic perovskite materials,[6–13] which have limitations such as high sintering temperatures, high heavy metal content, and complex preparation processes, all of which hinder their widespread use. Compared with inorganic materials, organic ferroelectric materials have the advantages of chemical stability, non-toxicity, no need for high-temperature heat treatment in the film-forming process, high flexibility, and low energy consumption.[14–17] As a result, many new organic ferroelectric materials have been developed, including polyvinylidene fluoride (PVDF) and its copolymers, organic polymer composites, and so on.[18] Among these, PVDF and its derivatives have attracted considerable attention due to their outstanding ferroelectric, piezoelectric, and pyroelectric properties, as well as their excellent ductility and stable chemical behavior.[19–21]

    PVDF is a crystalline polymer that consists of repeating monomers of polyethylene (–CH2–CH2–) and polytetrafluoroethylene (–CF2–CF2–). Its ferroelectricity arises from the electronegativity difference between the hydrocarbon and fluorine atoms.[22] There are typically four crystal forms: α-, β-, γ-, and δ-phases. The α-phase is the most stable, featuring a torsional molecular structure, as shown in Fig. 1. In this phase, the dipoles within the same unit cell are reversed, resulting in the cancellation of dipole moments, making the α-phase non-polar.[23] The β-, γ-, and δ-phases all exhibit polarity, with the γ- and δ-phases showing very weak polarity. The β-phase adopts an all-trans configuration, where carbon atoms form a Z-shaped skeleton, and fluorine and hydrogen atoms are located on opposite sides of the carbon chain. Most electrons are attracted to the fluorine atoms, creating a dipole moment between the fluorine and hydrogen atoms. In this phase, the dipole moments in each unit cell are aligned in the same direction, resulting in a strong overall polarity.[24,25]

    Furthermore, researchers have found that introducing trifluoroethylene (TrFE) into the PVDF carbon chain significantly enhances the ferroelectric properties of the resulting polymer, P(VDF-TrFE).[26,27] The rotation barrier between TrFE and VDF prevents the molecular chain from adopting a helical structure, and as a result, P(VDF-TrFE) forms an all-trans configuration due to steric hindrance. Figure 2 illustrates the structure formed by the incorporation of TrFE.

    The ferroelectric properties of materials and their polarization inversion mechanisms are crucial for their practical applications. Properties such as capacitance, piezoelectricity, and dielectric constant are closely linked to the polarization state of ferroelectric materials. Understanding the polarization reversal mechanism allows for the optimization of these properties, enhancing material performance in various applications. For instance, in memory devices, fast and stable polarization reversal can significantly improve read/write speed and data retention.[28–30] A thorough understanding of the specific mechanism and dynamic process of polarization reversal can inform the design and manufacturing of ferroelectric materials. By adjusting factors such as composition, structure, and external conditions (e.g., temperature and electric field), the polarization reversal process can be precisely controlled, thereby enhancing the reliability and lifespan of devices.[31,32]

    Ferroelectric materials are also widely utilized in fields such as sensors, actuators, energy harvesting, and non-volatile memory. A deeper understanding of the polarization reversal mechanism can facilitate the advancement of these materials in emerging fields, including flexible electronics, wearable technologies, and next-generation computing systems. In practical applications, however, the depolarization effect can degrade material properties. Studying the polarization reversal mechanism is essential for developing materials that resist depolarization and maintain long-term stability.[33–35] The polarization reversal process in PVDF has been extensively studied,[36–42] and the dynamics of ferroelectric inversion are typically described by the Kolmogorov–Avrami–Ishibashi (KAI) model developed by Ishibashi and Takagi, which is based on classical statistical theory of nucleation and unlimited domain growth, as formulated by Kolmogorov and Avram,[43–45]

    where ΔP(t) represents the change in polarization with time, Pr is the saturation polarization intensity, and t0 is the characteristic switching time. In the traditional KAI method, the Avrami index n is dependent on the dimension of the field and takes only integer values. For a single crystal, the index is 3, while for an epitaxial film, it is 2. However, for polycrystalline films, experimental practices typically either constrain the Avrami index n to a value of 2 or treat it as an arbitrary fitting parameter. In addition, non-KAI mechanisms have also been reported.[46–49]

    The microstructure of PVDF is influenced by factors such as molecular weight, molecular weight distribution, and processing conditions, including the solvent used and annealing protocols. Defects and structural disorders further complicate the material’s properties.[50] As a result, the mechanisms of spontaneous polarization, ferroelectric switching, and phase transitions remain unclear. The development of new ferroelectric materials is still highly empirical, as many of these mechanisms cannot be derived from first principles due to the large number of atoms involved, and the complexity of the molecular crystal structure. This presents a significant challenge to first-principles calculations.

    Molecular dynamics (MD) simulations are a powerful tool for modeling large systems containing millions of atoms,[51] but their accuracy is heavily influenced by the choice of force field parameters. In classical force fields such as AMBER and CHARMM,[52,53] the electrostatic interactions are primarily described by Coulomb interactions between fixed partial charges on atoms. However, these models are limited in their ability to simulate molecular crystals accurately, as they do not account for electric polarization.[54,55] As a result, directly applying force field-based MD simulations to molecular ferroelectrics is problematic.

    The exploration and validation of these mechanisms remain critical challenges in the study of molecular ferroelectrics. To address these issues, Li’s research group recently developed the polarized crystal charge (PCC) model, which incorporates the essential quantum electric polarization effect into molecular crystal simulations.[54] This model enables efficient and accurate simulations of molecular ferroelectrics.[56–58] This study systematically elucidates the ferroelectric switching and thermally induced phase transition dynamics processes of small-scale P(VDF-TrFE) under an applied electric field using the PCC model combined with molecular dynamics simulations. The mechanisms of ferroelectric switching and the ferro-/paraelectric phase transition were revealed, providing valuable guidance for the future design of organic molecular ferroelectrics and promoting their applications in industrial production and everyday life.

2.   Conputational detail and methods
  • The original molecular structure of PVDF was obtained from the Cambridge Crystallographic Data Centre (CCDC) database,[59] with entry ID 1293984, and was optimized using the Vienna Ab-initio Simulation Package (VASP) package.[60] The atomic replacement was then performed to generate the P(VDF-TrFE) (7:3) copolymer. The optimized configuration was selected as the initial structure for the molecular dynamics simulation. A 2 × 2 × 30 supercell, with dimensions 17.140 Å × 9.9 Å × 75.600 Å, was constructed. The polarization of P(VDF-TrFE) is evaluated using density functional theory (DFT). All calculations were performed using the Perdew–Burke–Ernzerhof (PBE) exchange–correlation functional and the project-augmented wave (PAW) method.[61,62] The calculations used a 1 × 1 × 1 Monkhorst–Pack K-point grid, and the plane wave cutoff was set to 400 eV. The Berry phase method was employed to calculate the electric dipole moment, and the polarization intensity was obtained by dividing the electric dipole moment by the volume.[63]

    GROMACS was used for the molecular dynamics simulations, and most parameters were obtained from the Generalized Amber Force Field (GAFF).[64,65] A new charge model, the PCC model, was applied to evaluate the partial charges, incorporating the quantum electric polarization effect of atoms in different molecules.[56] In the force field currently in use, atomic interactions are mainly divided into electrostatic interactions and van der Waals interactions, with the latter being approximated by fixed charges and classical Lennard–Jones (LJ) potentials. The PCC model, based on the RESP (Restrained Electrostatic Potential) point charge approach, accounts for the electrostatic effects of the environment on the charge distribution in the molecular while also considering the influence of other molecules in the system on the electron cloud distribution.

    Firstly, the background interference is eliminated, and the initial charge is obtained by the RESP charge fitting method.[66,67] The resulting charge is then added to the background. After several cycles of calculation, the charge converges, and the converged charge represents the exact atomic charge. The atomic charges obtained through these steps accurately reflect the electronic structure of the system after dynamic simulation and are proven to be suitable for simulating molecular crystals.[56–58]

    The PCC charge is calculated using the Gaussian software package,[68] with partial results presented in Table 1. Figure 3 illustrates the differences calculated between every two convergences.

    In order to investigate the polarization switching mechanisms of P(VDF-TrFE), molecular dynamics simulations were carried out under various temperatures and applied electric field conditions. Topological files were generated using the Sobtop production tools.[69] The leap-frog integrator was employed in the MD simulations,[70] with a time step of 1 fs and a total of 100 thousand simulation steps, corresponding to a simulation time of 100 ps. The LINCS algorithm was used to constrain all hydrogen bonds, with the number of iterations set to 2 and the algorithm’s order set to 4,[71] ensuring the precision and stability of the constraints. For processing non-bonded interactions, the Verlet truncation scheme was used to construct the neighbor list,[72] and the list was updated every 10 steps. The particle mesh Ewald (PME) method was applied for charge interactions,[73] with a short-range truncation radius set to 1.0 nm. Similarly, for van der Waals interactions, the short-range truncation radius was set to 1.0 nm, and dispersion corrections were applied to the energy and pressure calculations. Temperature coupling was achieved using the Nose–Hoover thermostat,[74] with the entire system treated as a coupled group. The simulation was performed under constant temperature (canonical ensemble, NVT),[75] with periodic boundary conditions applied in all directions (XYZ). The initial velocities were generated according to the Maxwell–Boltzmann distribution for the given temperature,[76] and random seeds were used for velocity initialization.

3.   Results and discussion
  • To investigate the ferroelectric properties of P(VDF-TrFE), we first examined the crystal structure and polarization changes under the application of an electric field E at 50 K.

    For this study, we focused exclusively on the β-phase. The electric field direction was aligned along the b-axis (the y-direction in our model). The hysteresis loop consists of two parts: the first part involves increasing the electric field from 0 V/nm to 10 V/nm and then reversing it to −10 V/nm; the second part involves decreasing the electric field from 0 V/nm to −10 V/nm and then reversing it back to 10 V/nm. The results of these simulations are shown in Fig. 4.

    It is obvious that P(VDF-TrFE)(7:3) forms a fully arranged ferroelectric molecular structure at about 3.5 V/nm and achieves saturation polarization with a saturation polarization value of about 5.3 μC/cm2. Other experimental studies report polarization values in the range of 5 μC/cm2–8 μC/cm2,[77,78] depending on factors such as material orientation, temperature, and testing methods. The simulation was conducted at a relatively low temperature, where dipole alignment tends to be more stable, resulting in a slightly lower saturation polarization value. Additionally, the simulation model is based on a small-scale system, lacking common features in experimental samples such as grain boundaries, defects, or polycrystalline characteristics, which may lead to a slightly lower simulated value compared to experimental results. This trend is consistent with Zhao et al.’s research.[42] When the direction of the electric field E is changed, the polarization will be reversed, and the coercive field is about 0.5 V/nm. The residual polarization of the system is low. A polarization intensity of 5.3 μC/cm2 is sufficient to meet the requirements of non-volatile memory devices and sensors, while being easier to process and integrate compared to inorganic ferroelectrics. The moderate polarization value suggests low-power switching characteristics, making it ideal for low-voltage-driven microelectronic devices. Furthermore, the low residual polarization observed in the simulation indicates excellent polarization switching capability, making the material suitable for applications requiring fast response and high durability, such as ferroelectric field-effect transistors.[79]

    The ferroelectric hysteresis loop obtained from molecular dynamics simulations exhibits certain fluctuations in the transition region, which may be attributed to finite-size effects, statistical noise, or the intrinsic characteristics of nanoscale ferroelectric switching. The shape of the hysteresis loop is influenced by multiple factors. In macroscopic ferroelectric materials, domain nucleation and domain wall motion play a significant role in polarization reversal, typically leading to broader and smoother hysteresis loops. However, in the nanoscale simulation system of this study, where domain walls are absent, polarization reversal primarily occurs through direct flipping of local dipoles, which may result in sharper transitions and less pronounced saturation effects compared to macroscopic systems. Additionally, periodic boundary conditions may enhance cooperative dipole switching, further affecting the shape of the hysteresis loop.

    Future studies could explore larger system sizes to reduce finite-size effects and further optimize sampling strategies, such as extending simulation time or increasing sampling frequency, to improve the convergence of data points and obtain a more refined hysteresis curve, thereby further verifying the ferroelectric behavior of P(VDF-TrFE).

    To investigate the switching mechanism furthe, we also analyze the change in polarization over time and fit the evolution of the spontaneous polarization to the KAI model. Figure 5 presents the polarization reversal diagram at different applied electric fields at 50 K, with the black curve representing the KAI fitting.

    Firstly, an external electric field is applied at 50 K to achieve saturation polarization, and then the direction of the electric field is reversed to calculate the change in polarization reversal over time. When an opposite external electric field is applied, it influences the dipole moment in the molecular chain. The chain is subjected to an opposing electric field force, which induces a reversal of the dipole direction. This flipping process involves the rearrangement of the local molecular structure, particularly the relative positioning of fluorine and hydrogen atoms relative to the carbon chain, which manifests as polarization reversal.

    The fitting results indicate that the switching mechanism deviates slightly from the KAI model, particularly in the time regions where polarization reversal begins and approaches saturation. However, in the asymptotic and switching regions, the data closely follow the predictions of the KAI model. The KAI model assumes a slow nucleation process in the initial stage, where polarization switching occurs through the gradual expansion of randomly nucleated regions. Consequently, it predicts a slower initial response. In contrast, the simulated system is based on a small-scale model, which features lower energy barriers compared to experimental polycrystalline systems. The small-size effect and periodic boundary conditions make the dipoles within the system more susceptible to electric field influence, resulting in a slightly faster switching process at the beginning. In the asymptotic and switching regions, the primary mechanism involves the ordered alignment of neighboring dipoles, which is consistent with the polarization growth process described by the KAI model. Near the saturation stage, however, the simulated polarization switching level is slightly lower than the saturation value predicted by the KAI model. This discrepancy may be attributed to local defects, thermal fluctuations in dipole orientations, or residual polarization caused by finite-size effects.

    The fitted Avrami index n are 1.21, 1.09, 1.49, and 1.44, all of which fall between 1 and 2, consistent with previous reports.[42] In experiments, typical ferroelectric materials exhibit polarization switching times on the nanosecond scale.[80,81] However, in nanoscale thin films or interfacial materials, the switching time can be further reduced to the picosecond scale.[82,83] In this simulation, polarization switching is completed within approximately 10 ps, demonstrating high-speed dynamic behavior. The simulation employs a small-scale system, which lacks the grain boundaries and defects commonly found in experimental systems. This reduces the energy barriers for dipole flipping and may lead to cooperative switching of dipoles, where multiple dipoles reverse simultaneously rather than sequentially. This collective behavior significantly accelerates the polarization switching process. Such a fast response outperforms traditional nanosecond-scale devices, showing great potential for high-speed memory applications.

    To better understand the significance of these results, we compared the polarization switching dynamics of P(VDF-TrFE) with PVDF and other ferroelectric polymers. PVDF is a widely studied ferroelectric polymer, and its polarization switching dynamics are generally slower than those of P(VDF-TrFE). This difference primarily arises from the stronger intermolecular interactions in PVDF, which result in a higher energy barrier for dipole flipping. Consequently, the polarization switching time of PVDF is typically in the nanosecond range. With the introduction of trifluoroethylene (TrFE), the backbone of PVDF undergoes a structural change, where the helical conformation is disrupted and the all-trans configuration is stabilized, thereby reducing the rotational energy barrier for dipole reorientation. This structural modification promotes cooperative dipole flipping, enabling P(VDF-TrFE) to achieve faster polarization switching compared to pure PVDF.[26,27] Furthermore, compared to other similar ferroelectric copolymers such as P(VDF-CTFE) and P(VDF-HFP), P(VDF-TrFE) does not exhibit relaxor ferroelectric behavior. These characteristics make P(VDF-TrFE) more suitable for high-speed, low-power ferroelectric memory devices and sensor applications.

    While molecular dynamics (MD) simulations provide valuable insights into the ferroelectric behavior of P(VDF-TrFE) at the atomic scale, certain limitations must be acknowledged.

    First, MD simulations are inherently constrained by the accuracy of the employed force field. In this study, the Generalized Amber Force Field (GAFF) was used in conjunction with the PCC model to describe interatomic interactions. However, classical force fields may not fully capture complex quantum effects, such as electron delocalization and polarization fluctuations, which could impact the accuracy of polarization dynamics predictions.

    Additionally, the finite size of the simulation box and periodic boundary conditions may introduce artifacts. For instance, nanoscale models lack grain boundaries, defects, and domain wall motion, leading to polarization switching dynamics that may differ from those in bulk materials. These effects could influence the estimated coercive field and switching speed, making direct comparisons with experimental macroscopic systems challenging. Future studies could improve accuracy by employing larger system sizes, refined force fields, and first-principles calculations to further validate these findings.

    The PCC method, which is used to evaluate atomic partial charges, also relies on certain assumptions. It is based on the RESP fitting method, which assumes a fixed charge distribution for a given molecular configuration. However, in real materials, charge redistribution occurs dynamically due to external perturbations such as electric fields and thermal fluctuations. Although the PCC model improves upon traditional fixed-charge approaches by incorporating environmental polarization effects, it does not fully account for dynamic charge transfer or long-range many-body interactions. Future work could explore polarizable force fields or hybrid quantum-classical (QM/MM) methods to refine the description of electronic polarization effects in P(VDF-TrFE).

    In practical applications, ferroelectric properties are typically required to remain stable within a certain temperature range. To investigate this, we also use MD simulations to study the phase transition temperature of the P(VDF-TrFE) ferroelectric phase over the temperature range of 50 K–500 K. In Fig. 6(a), the curves of different colors represent the polarization intensity at different times for various temperatures. Figure 6(b) shows the variation of the mean polarization intensity with temperature.

    At temperatures ranging from 50 K to 420 K, molecular dipoles are strongly constrained by the crystalline field, resulting in an ordered arrangement and exhibiting ferroelectric behavior. The polarization intensity fluctuates between 4.5 μC/cm2 and 5.5 μC/cm2 in this temperature range. As the temperature increases to between 420 K and 430 K, thermal vibrations intensify, disrupting the ordered alignment of dipoles and ultimately leading to paraelectric behavior. This behavior is consistent with previously reported phase transitions occurring between 395 K and 413 K.[84–86] The system maintains ferroelectric performance over a wide temperature range, demonstrating excellent thermal stability. The observed fluctuations in polarization intensity may be attributed to the influence of thermal vibrations on the molecular dipoles, however, the overall alignment remains governed by the crystalline field. For practical applications, such as memory devices or sensors, ferroelectric materials must exhibit stable polarization performance across a broad temperature range. These simulation results confirm that P(VDF-TrFE) demonstrates the potential for application in environments ranging from room temperature to 420 K. Furthermore, the relatively high phase transition temperature highlights the material’s excellent thermal stability, making it suitable for use in electronic devices operating under high-temperature conditions.

    In this study, the phase transition temperature of P(VDF-TrFE) was estimated based on direct MD simulations at different temperatures. While this approach provides an intuitive evaluation of polarization stability, it has certain limitations due to finite sampling time and the presence of energy barriers between ferroelectric and paraelectric states.

    To overcome these limitations, enhanced sampling techniques such as metadynamics and adaptive biasing force methods can be employed. These techniques enable efficient crossing of energy barriers, allowing for a more comprehensive exploration of the free energy landscape and a more accurate prediction of the phase transition temperature. Additionally, the weighted histogram analysis method can be used to construct a statistically robust polarization-temperature curve, further refining the estimation of the transition point. Enhanced sampling methods can reduce the residence time of the system in metastable traps and enable more extensive exploration of the configurational space, which may adjust the estimated phase transition temperature to be closer to the experimentally reported range (395 K–413 K). Compared to the conventional simple two-state transition, enhanced sampling may reveal intermediate states between ferroelectric and paraelectric phases, which may involve transient short-range ordered structures. Given the molecular nature of P(VDF-TrFE), such a transition process is likely to be more complex than that in conventional crystalline ferroelectrics. By improving sampling efficiency, these methods can also mitigate artifacts introduced by finite system size and periodic boundary conditions, leading to a more intrinsic evaluation of the phase transition properties of nanoscale P(VDF-TrFE).

    Future studies could integrate these advanced enhanced sampling techniques to gain deeper insights into the phase transition behavior of P(VDF-TrFE) and improve the predictive accuracy of its ferroelectric stability.

4.   Conclusion
  • In summary, we used the polarized crystal charge molecular dynamics method to simulate the ferroelectric switching mechanism of P(VDF-TrFE)(7:3) under an applied electric field. The simulation results include the spontaneous polarization, coercive field, ferroelectric hysteresis loop, and the corresponding switching mechanism. We found that under an applied electric field of approximately 3.5 V/nm, the fully aligned ferroelectric molecular structure achieved saturation polarization, with a value of about 5.3 μC/cm2, which is consistent with experimental trends. The coercive field was approximately 0.5 V/nm. The low residual polarization observed in the simulations suggests excellent polarization switching capability, making this material well-suited for applications requiring fast response and high durability. Moreover, the polarization reversal dynamics in the asymptotic and switching regions closely follow the KAI model, with the Avrami index matching theoretical predictions. The polarization reversal process was completed within approximately 10 ps, demonstrating high-speed dynamic behavior.

    Additionally, the thermally induced phase transition dynamics processes were also simulated. The ferroelectric phase transition of P(VDF-TrFE) is predicted to occur in the temperature range of 420 K–430 K, which closely aligns with the experimental value and is near the material’s melting point. Our simulation results demonstrate that nanoscale P(VDF-TrFE) exhibits low-power switching characteristics and excellent polarization switching capabilities, making it an ideal candidate for low-voltage-driven microelectronic devices, as well as applications requiring fast response and high durability. Furthermore, it maintains ferroelectric performance over a wide temperature range and shows a high phase transition temperature, indicating exceptional thermal stability, which is advantageous for practical applications. Additionally, this study expands the applicability of the PCC molecular dynamics method in the investigation of organic molecular ferroelectrics. It is hoped that these findings will provide a useful foundation for further research on organic ferroelectric materials and their potential applications in modern electronic and energy storage devices. as

Figure (6)  Table (1) Reference (86)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return