2025 Volume 34 Issue 6
Article Contents

Zheng-Yi Liao, Pai-Wen Fang, Xing Lu, Gang Wang, Yan-Li Pei. Low leakage current β-Ga2O3 MOS capacitors with ALD deposited Al2O3 gate dielectric using ozone as precursor[J]. Chinese Physics B, 2025, 34(6): 067304. doi: 10.1088/1674-1056/adc660
Citation: Zheng-Yi Liao, Pai-Wen Fang, Xing Lu, Gang Wang, Yan-Li Pei. Low leakage current β-Ga2O3 MOS capacitors with ALD deposited Al2O3 gate dielectric using ozone as precursor[J]. Chinese Physics B, 2025, 34(6): 067304. doi: 10.1088/1674-1056/adc660

Low leakage current β-Ga2O3 MOS capacitors with ALD deposited Al2O3 gate dielectric using ozone as precursor

  • Received Date: 15/01/2025
    Accepted Date: 25/03/2025
    Available Online: 01/06/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(7)  /  Tables(1)

Article Metrics

Article views(948) PDF downloads(4) Cited by(0)

Access History

Low leakage current β-Ga2O3 MOS capacitors with ALD deposited Al2O3 gate dielectric using ozone as precursor

Abstract: Metal–insulator–semiconductor (MOS) capacitor is a key structure for high performance MOS field transistors (MOSFETs), requiring low leakage current, high breakdown voltage, and low interface states. In this paper, β-Ga2O3 MOS capacitors were fabricated with ALD deposited Al2O3 using H2O or ozone (O3) as precursors. Compared with the Al2O3 gate dielectric with H2O as ALD precursor, the leakage current for the O3 precursor case is decreased by two orders of magnitude, while it keeps the same level at the fixed charges, interface state density, and border traps. The SIMS tests show that Al2O3 with O3 as precursor contains more carbon impurities. The current transport mechanism analysis suggests that the C–H complex in Al2O3 with O3 precursor serves as deep energy trap to reduce the leakage current. These results indicate that the Al2O3/β-Ga2O3 MOS capacitor using the O3 precursor has a low leakage current and holds potential for application in β-Ga2O3 MOSFETs.

1.   Introduction
  • The β-Ga2O3 with an ultrawide bandgap of ∼4.8 eV features a high theoretical breakdown electric field of 8 MV/cm and strong radiation resistance, making it potential for high-voltage power electronic device.[1–4] Metal–oxide–semiconductor field-effect transistors (MOSFETs) are very important power electronic device with the ability to handle high voltages and large currents. Recently, high breakdown voltage and low on-resistance β-Ga2O3-based planar and vertical MOSFETs have been reported, highlighting their potential in high-power electronics.[5–7] However, there is still a lot of room for improvement in performance. The high-quality dielectric/β-Ga2O3 capacitor is significantly important for fabricating high-performance MOSFETs, which should exhibit low leakage currents and stable electric field dividing,[8,9] requiring dense oxide film with lower oxide fixed charges and border traps, and good interface between the dielectric and semiconductor with lower interface states density (Dit).

    Various dielectric materials such as Al2O3,[10–15] HfO2,[16–18] SiO2,[19,20] and HfAlO[21,22] are studied for β-Ga2O3-based MOS capacitors. Among these dielectric materials, the atomic layer deposition (ALD) Al2O3 and its double-layer such as Al2O3/HfO2, have been widely studied due to its high-precision layer-by-layer deposition process, large conduction band offset with β-Ga2O3 (1.5 eV–2.2 eV),[8,9] and high relative permittivity. The ALD Al2O3 in the above studies were deposited using tri-methyl-aluminum (TMA) and H2O as precursor. We noticed that a number of ALD Al2O3 studies in the past have utilized using ozone (O3) as an oxygen precursor deposited on Si and other semiconductors, which has resulted in lower leakage current levels and larger breakdown voltages.[23–25] However, β-Ga2O3-based MOS capacitors using ALD Al2O3 deposited with O3 as a precursor have not been systematically studied. In this work, we systematically investigate β-Ga2O3-based MOS capacitors with ALD Al2O3 gate dielectric using O3 or H2O as precursors. The O3 precursor-based Al2O3/(–201)β-Ga2O3 MOS capacitors show significantly lower leakage current than those commonly using H2O precursor, as well as the same level in the breakdown voltage, fixed charges, border traps, and interface states density. The possible physicochemical mechanisms are discussed in this study.

2.   Experiments
  • Sn-doped (–201) β-Ga2O3 substrates with a carrier density of ∼ 2 × 1017 cm−3 were ultrasonic cleaned in methanol and acetone, and then soaked in SPM solution (de-ionized water:30% H2O2:96% H2SO4 = 1:1:4) to remove organic and metal pollution. Afterwards, the substrates were treated with piranha (98% H2SO4:30% H2O2 = 3:1) for 1 min to hydroxylate the β-Ga2O3 surface. Immediately after surface treatment, the β-Ga2O3 substrates were transferred to the ALD chamber. 20-nm thick Al2O3 films were deposited at 200 °C using tri-methyl-aluminum (TMA) and O3 or H2O as precursors. The pulse times for TMA and H2O are 20 ms, while for ozone, the pulse time is 500 ms. All purge times are set to be 20 s by N2. ozone is generated by introducing 5N oxygen into an ozone generator. The actual ozone concentration is below 10%, and it will further decrease when the gas is introduced into the chamber. The gas flow rate is set to be 50 sccm. For convenience, the Al2O3 thin films deposited using O3 or H2O as precursors are denoted as O3–Al2O3 and H2O–Al2O3, respectively. In order to determine the chemical composition of Al2O3 thin films, secondary ion mass spectrometry (SIMS) was used to analyze the depth distribution of H, C, O, Al, and Ga elements in the stack of Al2O3/β-Ga2O3 structure.

    The MOS capacitors’ structure was shown in Fig. 1(a). Ti/Al/Ni/Au(15/80/20/60 nm) were deposited using electron beam evaporation and annealed with rapid thermal annealing for 1 min at 470 °C under N2 atmosphere to form Ohmic contact. Ti/Au (20/80 nm) anodes were then fabricated by lift-off process. Capacitance–voltage (C–V) and current–voltage (I–V) characteristics were measured by semiconductor analyzer Agilent B1500.

3.   Results and discussion
  • The C–V measurement results of Al2O3/(–201)β-Ga2O3 MOS capacitors are shown in Fig. 2. The curves with dash line are the Silvaco simulation results. The DC voltage for the C–V test was set from −2 V to 5 V, with a sweeping step of 50 mV and the sweeping frequency of 1 kHz. The oxide capacitance Cox as the maximum accumulated capacitance is extracted from the first sweep scanning of C–V. They are Cox[H2O] = 0.37 μF/cm2 and Cox[O3] = 0.38 μF/cm2, for H2O–Al2O3 and O3–Al2O3, respectively. The relative permittivities of the two kinds of Al2O3 can be calculated by the equation as follows:

    where ε0 is the absolute permittivity with a value of 8.854 × 10−14 F/cm, A is anode area, d is the thickness of the Al2O3 extracted by ellipsometry. The relative permittivity is calculated as εr[H2O–Al2O3] = 8.36, εr[O3–Al2O3] = 8.58, which are summarized at Table 1. The both values are within the range of commonly studied values (8–9), indicating that the Al2O3 films deposited in this experiment are of good quality. During C–V measurements, we found that the C–V curves were continuously shifted to the positive direction with the number of sweeps, and finally stabilized after several sweeps, indicating that the electrons were trapped by the boundary traps Nbt in the Al2O3. The flat-band voltage Vfb was extracted from the (Cox/C)2 − 1 ∼ VG curve,[26] as shown in the insert of Fig. 2. The measured Vfb of the devices are shifted in the positive direction compared to the simulation curves due to the negative fixed charges existed in the Al2O3 layer. From the first sweep C–V curve and the finally stable curve, we extracted the shift of Vfb (ΔVfb). The curve of the ΔVfb versus sweep counts is supplemented in Fig. S1 of supplementary materials. It demonstrates that the CV curve stabilizes after several sweeps. The device with H2O–Al2O3 has a lower ΔVfb of 2.65 V compared to 3.31V of the O3–Al2O3 device.

    The fixed oxide charges Not and border trap Nbt are calculated by the following equations:[27–30]

    where Cox is dielectric capacitance equivalent to the accumulation capacitance of MOSCAP, ϕms is the difference in work function between titanium and β-Ga2O3, q is quantity of electron charge, and A is the anode area. As shown in Table 1, the border trap density of O3–Al2O3 MOS capacitor is increased by 28% and the fixed oxide charge density is increased by 13% compared with the H2O–Al2O3 MOS capacitor, which suggests that the O3 precursor leads to more charges and traps in the Al2O3 deposition process. However, we also should notice that for H2O–Al2O3 and O3–Al2O3, the fixed charges and border traps are the same level.

    Figures 3(a) and 3(b) show the C–V curves at different frequencies. From the results, we can calculate the interface states density Dit by high-low frequency method. The equation is as follows:[31,32]

    where CLF and CHF are the capacitances measured at frequency of 1 kHz and 1 MHz, respectively. The Dit (at Ec–Et = 0.6 eV) are 3.34 × 1011 cm−2⋅eV−1 and 2.64 × 1011 cm−2⋅eV−1 for O3–Al2O3 and H2O–Al2O3 capacitors, respectively. As shown in Fig. 3(c), O3–Al2O3 MOS capacitor has more interface states than H2O–Al2O3 MOS capacitor. However, both devices obtain a favorable interface which is necessary for high performance electronics devices.

  • Figure 4(a) shows the current density versus voltage curves (J–V) of the MOS capacitors. We found that compared with the H2O–Al2O3 capacitor, the leakage current of the O3–Al2O3 capacitor is lower by two orders. The properties make O3–Al2O3 a preferred choice for gate dielectric of β-Ga2O3 devices.

    In order to find the reason for low leakage current in O3–Al2O3 capacitor, the current conduction mechanism was analyzed. As shown in Fig. 4(b), when electric field (E) is less than 1.6 MV/cm for H2O device and 2.5 MV/cm for O3 device, the fitting curve conforms to a linear law. The results indicate that Ohmic injection caused by thermo-electronic emission is the main conduction mechanism until the electric field increases to the point where traps and charges begin to affect current conduction.[32–34] For H2O device, in the range of 1.7 MV/cm < E < 2.7 MV/cm, the conduction mechanism is Poole–Frenkel (PF) model, fitting by temperature dependence J–V curve as shown in Figs. 5(a) and 5(b). The expression of the PF model is given by[33–35]

    where qϕt is the trap energy level, εr is the relative permittivity, ε0 is the vacuum permittivity, and C1 is a constant. qϕt extracted from the curves are 0.04 eV–0.30 eV, indicating the shallow energy level trap in H2O–Al2O3. In contrast, as shown in Fig. 5(c), the J–V curve of O3 device is independence on the temperature so that it does not fit the PF model.

    As shown in Fig. 6(a), when at E > 3.1 MV/cm for H2O device and E > 3.4 MV/cm for O3 device before breakdown, trap-assisted tunneling (TAT) is dominant conduction mechanism which is virtually temperature-independent. The curves of both H2O and O3 devices can fit the model expressed by[33–35]

    where m* is effective electron mass in Al2O3, h is Plancks’ constant, ϕT is trap energy level below the oxide conduction band, and C2 is a constant. The value of m* is set as 0.28m0,[36] where m0 is the free electron mass. By performing linear fitting on the temperature-independent regions of the characteristic curves, the slope and ϕT values are extracted. The ϕT value is ∼ 1.20 eV for O3 device which is larger than ∼ 0.84 eV for H2O device, as shown in Fig. 6(a). The trap energy level will affect the current transport, as shown in Figs. 6(b) and 6(c). The shallow energy level traps in H2O–Al2O3 lead to PF emission at low electric field and electron tunneling easily at high electric field. In contrast, the electron tunneling is harder in O3 device with the deep energy level traps resulting in lower leakage current in the same electric field. Additionally, the deep energy level traps of O3-device also account for its non-compliance with the PF emission model, since the electrons are difficult to be thermally emitted from the deep energy level into the conduction band as shown in Fig. 6(c).

    In order to elucidate the origin of the distinct conduction mechanisms between the two devices, we conducted a comparative analysis of chemical compositions for H2O–Al2O3 and O3–Al2O3 dielectric layers. Figure 7 shows the SIMS results. The elements of H, C, O, Al, and Ga were profiled as the depth from the top surface of Al2O3 to the β-Ga2O3 substrate at a total of 60 nm. The C and H as impurities were quantitatively analyzed. The SIMS test results show that the C concentration of O3–Al2O3 is remarkably higher than that of H2O–Al2O3, while the H concentration of both is similar. In general, the reaction of TMA with H2O or O3 produces different by-products, leading to the different C concentrations.[37,38] It has been reported that H is a shallow energy level defect in ALD–Al2O3 which is related to the oxide conductivity[39] and that the C impurity in ALD–Al2O3 would be passivated by H, forming a C–H complex with deep energy level.[40] Combined with experimental results, we suggest that the C–H impurities in O3–Al2O3 lead to deep energy level traps and low leakage compared to the H2O–Al2O3 with H impurities. Additionally, based on the previous C–V analysis, we speculate that the C impurities also contribute to the charges in Al2O3, which requires further research.

4.   Conclusion
  • The β-Ga2O3 MOS capacitors with ALD deposited Al2O3 using O3 or H2O as precursors were investigated. The leakage current for the O3–Al2O3 capacitor is decreased by two orders than the H2O precursor case, although the capacitors with Al2O3 using H2O as precursor have advantages in fixed charges, interface states density, and border traps. The current transport mechanisms were analyzed by fitting J–V curves and the results show that the deep energy level traps are in O3–Al2O3, leading to the reduced leakage current than the H2O–Al2O3 device with shallow energy level traps. The SIMS test shows that O3–Al2O3 contains more C impurities, which suggests deep energy level traps presumably are the C–H complex. Considering the same level in fixed charges, interface states density, and border traps, the O3 precursor-grown ALD Al2O3 has low leakage properties that are highly favorable for process applications in β-Ga2O3 power devices.

Figure (7)  Table (1) Reference (40)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return