Tingting Wei, Jinling Yu, Zhu Diao, Zhaonan Li, Shuying Cheng, Yunfeng Lai, Yonghai Chen, Chao Zhao. In-plane optical anisotropy of InGaN/GaN quantum disks in nanowires investigated by reflectance difference spectroscopy[J]. Chinese Physics B, 2025, 34(6): 067302. doi: 10.1088/1674-1056/adc6f4
Citation: Tingting Wei, Jinling Yu, Zhu Diao, Zhaonan Li, Shuying Cheng, Yunfeng Lai, Yonghai Chen, Chao Zhao. In-plane optical anisotropy of InGaN/GaN quantum disks in nanowires investigated by reflectance difference spectroscopy[J]. Chinese Physics B, 2025, 34(6): 067302. doi: 10.1088/1674-1056/adc6f4

In-plane optical anisotropy of InGaN/GaN quantum disks in nanowires investigated by reflectance difference spectroscopy

  • Received Date: 27/12/2024
    Accepted Date: 10/03/2025
    Available Online: 01/06/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(5)

Article Metrics

Article views(738) PDF downloads(1) Cited by(0)

Access History

In-plane optical anisotropy of InGaN/GaN quantum disks in nanowires investigated by reflectance difference spectroscopy

Abstract: The in-plane optical anisotropy (IPOA) of c-plane InGaN/GaN quantum disks (Qdisks) in nanowires grown on MoS2/Mo and Ti/Mo substrates is investigated using reflectance difference spectroscopy (RDS) at room temperature. A large IPOA related to defect or impurity states is observed. The IPOA of samples grown on MoS2/Mo is approximately one order of magnitude larger than that of samples grown on Ti/Mo substrates. Numerical calculations based on the envelope function approximation have been performed to analyze the origin of the IPOA. It is found that the IPOA primarily results from the segregation of indium atoms in the InGaN/GaN Qdisks. This work highlights the significant influence of substrate materials on the IPOA of semiconductor heterostructures.

1.   Introduction
  • InGaN/GaN multi-quantum-well structures have been widely used in light-emitting diodes (LEDs), since their energy bandgap can be tuned by varying the indium (In) composition.[1] However, the large lattice mismatch between GaN and InN makes it difficult to grow high-quality InGaN crystals. Utilizing a nanowire structure can facilitate the relaxation of this mechanical strain. Additionally, layered transition metal dichalcogenides (TMDs) provide an effective solution to challenges related to lattice mismatch and heat dissipation.[2–5] One important property of nanowire structures is their optical anisotropy, which is closely related to the crystallographic orientation of the nanowires. Reflectance difference spectroscopy (RDS) is a powerful tool to investigate the optical anisotropy of semiconductor quantum wells due to its high sensitivity. RDS has been adopted previously to investigate the in-plane optical anisotropy (IPOA) in InxGa1−xAs/GaAs quantum wells induced by anisotropic interface structures[6] and indium atom segregation.[7] Recently, Sundin et al. revealed significant anisotropic optical properties in InGaN nanowires grown by molecular beam epitaxy, employing two-photon absorption and photoluminescence microscopy.[8] Meanwhile, Ries et al. identified negative polarization anisotropy in self-assembled InGaN nanostructures on GaN nanowires via polarization-dependent photoluminescence, attributing the effect to possible superlattice formation in indium-rich regions.[9] Although many works have been carried out to investigate the properties of InGaN quantum wells and nanowires,[10] there is no report on the IPOA of InGaN/GaN quantum disks (Qdisks) in nanowires by RDS.

    In this work, we investigate the IPOA of InGaN/GaN Qdisks in nanowires grown on MoS2/Mo and Ti/Mo substrates using RDS. Notably, a large IOPA is observed in samples grown on MoS2/Mo substrates. To comprehensively understand the origins of the IPOA, numerical calculations based on the six-band k ⋅ p method are performed. The results reveal that the observed IPOA primarily arises from the segregation of In atoms.

2.   Samples and experiments
  • We have investigated four InxGa1−xN/GaN Qdisks-in-nanowire samples, named samples A, B, C and D, respectively. The samples are grown by molecular beam epitaxy (MBE). Samples A and B are grown on MoS2/Mo substrates, and samples C and D are grown on Mo substrates coated with 500 nm of Ti. Figure 1(a) shows the structure of sample A, where the nanowires (NWs) are 8 pairs of InxGa1−xN-disk (3 nm)/GaN-barrier (12 nm) grown at a substrate temperature of 700 °C. The NWs are sandwiched between a 150-nm-thick Si-doped n-type GaN layer and a 50-nm-thick Mg-doped p-GaN layer. The structure of sample B is similar to that of sample A, except that there are no p-type GaN layers in sample B, as shown in Fig. 1(b). Sample C has the same layer stack as sample A and the only difference between them is the substrate material. The structure of sample D is similar to that of sample C, except that there is no p-type GaN capping layer on the nanowires and the nanowires are grown at a temperature of 480 °C. By stacking the p-type GaN layers in samples A and C, a comparison is made between sample A and sample B on the same substrate, as well as between sample C and sample D on the same substrate. The experimental results are analyzed to determine whether the additional p-GaN layer would introduce an extra IPOA. as shown in Fig. 1(d). The nanowires of samples A and B have an average diameter of 20–55 nm and a density of about 2.6 × 1010 cm−2. For samples C and D, the nanowire density is about 1 × 1010 cm−2 with a diameter of 40–60 nm. For more detailed information on the sample growth, please refer to Refs. [11,12].

    The IPOA of the samples is measured by RDS. The experimental setup of the RDS is the same as that used in Ref. [13]. Using the RDS, we can measure the relative reflectance difference between [110] and [11¯0] directions, i.e., Δr=2(r110−r11¯0)/(r110+r11¯0). Here r110 (or r11¯0) is the reflection coefficient of the sample when the incident light is polarized along the [110] (or the [11¯0]) direction. Luminescence properties of the samples are investigated by room temperature (RT) photoluminescence (PL) with a steady-state fluorescence spectrometer (FLS1000, Edinburgh Instruments). PL measurements are performed using an excitation laser of 405 nm.

3.   Results and discussion
  • The PL spectra measured at RT for samples A–D are shown in Fig. 2(a). One can see that there is a shoulder at the lower energy side of the main PL peak. To obtain the peak positions of the PL spectra, we use two Gaussian functions to fit the PL spectra and the fitting results are shown by the dashed lines in Fig. 2(a). The PL spectra of the samples can be resolved into high-energy and low-energy emission peaks, named peak H and peak L, respectively, through Gaussian fitting. Peak H, which corresponds to transitions taking place in the InGaN Qdisks, is clearly observed at 2.53 eV, 2.52 eV, 2.57 eV and 2.81 eV in samples A–D, respectively. Peak L observed in the four samples may be attributed to compositional fluctuations in the InGaN Qdisks.[14]

    Figure 2(b) shows the imaginary part of the RDS spectra of the samples measured at room temperature, which have been shifted vertically for clarity. The high-energy peak position (around 2.81 eV) in the RDS spectra of sample D is not clearly resolved, which may be attributed to insufficient intensity in the ultraviolet spectral range of the light source used in the experiment. It can be seen that the peaks of the RDS spectra show very large full width at half maximum (FWHM), which may be a result of compositional fluctuations of In in the InGaN Qdisks during sample preparation. Compositional fluctuations lead to variations in the band gap across different regions of the material, which in turn broaden the peaks in the RDS spectra. Compared to the RDS signals previously observed in GaAs/AlGaAs quantum wells, the FWHM of the RDS peak in the Qdisk geometry is approximately five times larger.[6] This broadening is likely attributed to the greater compositional fluctuation of In within the InGaN Qdisks. The light spot of the RDS set-up is about 5 mm × 8 mm and the measured RDS signal is the average IPOA value over the entire light spot region. Therefore, it is not possible to determine whether these fluctuations are uniform across the samples or vary locally from the RDS results. By conducting PL measurements, which use a laser spot with a diameter of 1 mm, at two different positions on sample B, we find that the PL peak positions from the two measurements are nearly identical, indicating that the compositional fluctuations in the sample are uniform across the sample.

    Solid arrows in Fig. 2(b) denote the positions of peak H observed in the PL spectra in terms of photon energy. Peak H is attributed to the interband transitions in the InGaN Qdisks. It is evident from Fig. 2(b) that samples A and B, which are grown on MoS2/Mo substrates, exhibit prominent anisotropic transition peaks, whereas samples C and D, grown on Ti/Mo substrates, show negligible or nearly absent IPOA for interband transitions. This phenomenon indicates that substrates have significant influence on the IPOA of InGaN Qdisks in nanowires. The intensity of the IPOA in sample A is at the same level as that in sample B, indicating that the additional p-type GaN capping layer in sample A does not introduce any extra IPOA.

    In the RDS spectra, one can observe large IPOA signals below the band gap of InGaN. Since we do not observe any IPOA signal from the substrates alone, this signal may be primarily attributed to defect or impurity states.[15] According to Refs. [16,17], lattice defects introduced during the epitaxial growth process generate sub-bandgap states in InGaN Qdisks. It has been reported that there exists a defect state with trap energy 0.7 eV below the conduction band of InGaN. Moreover, nitrogen vacancies (VN) in InGaN introduce defect states that have a trap energy state 0.26 eV below the conduction band edge.[17] These defect and impurity states may be responsible for the IPOA signal below the band gap of InGaN. Our samples exhibit a pronounced IPOA signal below the band gap, which has never been observed in GaAs/AlGaAs QWs or GaN thin films.

    To investigate the origin of the IPOA of the interband transitions in the InGaN/GaN Qdisks in nanowires, we apply the six-band k ⋅ p method to calculate the IPOA of these samples. The IPOA signal in our samples mainly comes from the mixing of light-hole, heavy-hole and the spin–orbit split-off (SO) bands induced by anisotropic strain, the interface anisotropic potential and the segregation of In atoms.[13] We take all these effects into account in our calculations. The hole-mixing Hamiltonian H′ due to anisotropic strain, the interface anisotropic potential and In atom segregation can be expressed as[18]

    Here,

    with the basis of |3/2,3/2〉, |3/2,−1/2〉, |3/2,1/2〉, and |3/2,−3/2〉. εxy is the anisotropic strain in the sample and D is the deformation potential constant of the valence band. P1 and P2 are the anisotropic interface potential parameters, describing the anisotropy strength at the upper and lower interfaces of the InGaN/GaN heterostructure, respectively. The theta function Θ indicates that hole mixing due to anisotropic interfaces only occurs at the interfaces. l1 (or l2) is the segregation length of In atoms in the lower (or upper) interface and z = ±w/2 is the location of the interfaces in the InGaN/GaN heterostructure. In an ideally symmetric quantum well, P1 and P2 are equal, reflecting the identical potential effect of the interfaces on the carriers. However, in practical quantum wells, factors such as compositional inhomogeneity, asymmetry between the upper and lower interfaces, and irregular arrangements of atoms at the interfaces may lead to differences between P1 and P2.

    To calculate the energy and the envelope wave function of holes, we use the 6 × 6 Lüttinger Hamiltonian HL and a hole-mixing Hamiltonian expressed in Eq. (1) based on the k ⋅ p method. On the other hand, the energy and the envelope wave function of electrons are calculated using the two-band k ⋅ p method. The band gap Eg of strain-free InxGa1−xN can be calculated as Eg (InxGa1–xN) = xEg (InN) + (1–x)Eg (GaN) – bx(1–x). Here, the reported band gap of InN, Eg(InN), is 0.64 eV and the band gap of GaN, Eg(GaN), is 3.43 eV. b is the bowing parameter that accounts for the nonlinear effect of the band gap, which takes the value of 2.8 eV.[19] The band alignment at the InGaN/GaN interface is type I and the band offset is taken as ΔEc/ΔEv = 0.7/0.3.[20] After performing numerical calculations based on the six-band k ⋅ p method, it is revealed that the first and third hole bands for the InGaN/GaN Qdisks are primarily heavy-hole bands. The second band, in contrast, is a mixing band of light holes and SO bands, which is denoted as the light-hole band for the convenience of discussion.

    After obtaining the energy and the envelope wave function of electrons and holes, we can calculate the average transition probability Pnm and the anisotropic transition probability ΔPnm. Here, Pnm is the transition probability between the nth sub-band of electrons and the mth sub-band of holes, defined as Pnm=(P110+P11¯0)/2 with P110 (or P11¯0) being the transition probability when the incident light is polarized along the [110] (or the [11¯0]) direction. ΔPnm is the anisotropic transition probability defined as ΔPnm=P110−P11¯0. Then, the average transition spectrum M and the anisotropic transition spectrum ΔM can be simulated using the Lorentzian function, which is described as[7]

    Here, Γ is the linewidth of the transition and Enm is the transition energy between the nth sub-band of electrons and the mth sub-band of holes. Parameters used in the calculation are deduced from Ref. [21], and a linear interpolation is adopted in the calculation of all parameters except for the band gap energy of InxGa1−xN.

    The IPOA in the InGaN/GaN Qdisks in nanowires primarily arises from the coupling among heavy-hole, light-hole and SO bands. This coupling may be driven by factors such as anisotropic strain, indium atom segregation, the anisotropic chemical bond arrangement at the interface and anisotropic interface structures.[13] Both the anisotropic chemical bond arrangement at the interface and the anisotropic interface structures can be described by the interface potential. According to the perturbed interface potential model (called “HBF”) proposed by Krebs,[22] the interface potential P0 can be estimated as a0ΔV43. Here, a0 is the lattice constant of InGaN and ΔV is the valence band offset at the interface. Thus, for the GaN/InN interface, the interface potential P0 is estimated to be 1823 meV⋅Å, while the interface potential for the GaN/InxGa1−xN interface is obtained by linear interpolation.

    If we only consider the effect of the interface potential, we have the segregation length l1 = l2 = 0 and the anisotropic strain εxy = 0. The interface potential P1 = P0⋅ x and P2 ≠ P1. Here, x is the In concentration. ΔP = P2 – P1 is used to characterize the degree of asymmetry between the upper and the lower interfaces. By comparing the calculated transition energy of 1H1E (i.e., the transition from the first heavy-hole sub-band to the first conduction band) with that obtained in the PL spectra, we can determine that the In concentrations of the InxGa1−xN Qdisks are approximately 0.21 for samples A, B and C, and only 0.145 for sample D. In this calculation, the anisotropic interface potential ΔP is assumed to be 0.02P1. For x = 0.21, ΔP is 12.7 meV⋅Å. This is a reasonable value for a quantum well (QW) structure with common atoms at the interface, given that ΔP is 16 meV⋅Å, for GaAs/AlGaAs, another QW structure with common atoms at the interface.[6] Simulation results with ΔP = 0.02 P1 are shown in Fig. 3.

    Figures 3(a) and 3(b) illustrate the dependence of the anisotropic transition probability induced by the interface potential and the transition energy for transitions 1H1E, 1L1E and 2H1E on the quantum well thickness in an In0.21Ga0.79N/GaN Qdisk, respectively. It can be seen that the anisotropic transition probability of transitions 1H1E and 1L1E decreases with an increase of the In0.21Ga0.79N thickness, while that of the 2H1E first increases and then decreases. In contrast, the transition energy of all three transitions decreases with the thickness of In0.21Ga0.79N. Figure 3(c) shows the dependence of the anisotropic transition probability induced by the interface potential of the same three transitions on the indium concentration (x) with the thickness of the InxGa1−xN layer fixed at 3 nm. It can be seen that the anisotropic transition probability of these transitions increases with the In composition. This can be attributed to the fact that as the increase of the In composition, the interface potential P1 increases and the interface potential difference between the two interfaces ΔP also increases. Figure 3(d) shows the calculated anisotropic transition spectrum ΔM with a linewidth Γ of 0.01 eV and 0.2 eV, respectively, induced by the interface potential for a 3-nm In0.21Ga0.79N/GaN Qdisk. We note that the IPOA of 1H1E and 1L1E shows almost equal amplitude but with opposite signs, and the transition energy of 1H1E and 1L1E is quite close to each other. As a result, under a large linewidth of 0.2 eV, the superposition of the ΔM peaks of 1H1E and 1L1E will lead to a significant reduction in the overall peak intensity, as shown in Fig. 3(d).

    If we only consider the effect of the anisotropic strain εxy, we adopt the following values in our calculation: the segregation length l1 = l2 = 0, the interface potential P1 = P2 = P0⋅ x and the anisotropic strain εxy ≠ 0. Anisotropic strain may be induced by different degrees of strain relaxation between the [110] and the [11¯0] axes. Additionally, at the InGaN/GaN interface, due to the different lattice parameters of InGaN and GaN, there will be a strain along the [110] or the [11¯0] axis, leading to a nonzero εxy. It is reasonable to assume that εxy is proportional to εxx. In our calculation, we assume εxy = 0.003εxx and the simulation results are shown in Fig. 4. It is worth mentioning that the reason for using εxy = 0.003εxx in the simulation is because by using such a value, the simulated IPOA is at the same order as the simulated IPOA induced by the interface potential or the In atom segregation effect. This value is also adopted in a previous report,[7] which is proved to be a reasonable value. It can be seen from Fig. 4(a) that, with the increase of the InGaN thickness in the InGaN/GaN Qdisk, the amplitude of the anisotropic transition probability of the 1H1E, 1L1E and 2H1E transitions does not show any significant changes. Comparing Fig. 4(b) with Fig. 3(b), we note that the transition energy of 1H1E, 1L1E and 2H1E under an anisotropic strain εxy = 0.003εxx is almost the same as that under an asymmetric interface potential ΔP = 0.02P1. It can be seen from Fig. 4(c) that the anisotropic transition probability of 1H1E, 1L1E and 2H1E increases with the In composition. As the In composition increases, the strain εxx increases, leading to an increase in εxy. Figure 4(d) indicates that for the 3-nm In0.21Ga0.79N/GaN Qdisk, the IPOA of the 1H1E and 1L1E transitions shows almost equal amplitude but with opposite signs. Under a large linewidth of 0.2 eV, the overall intensity of the IPOA is greatly reduced due to the overlap of the ΔM peaks of 1H1E and 1L1E. It can be seen that the IPOA induced by anisotropic strain is dominated by 1H1E, 1L1E and 2H1E.

    If we only consider the In atom segregation, the following parameters are adopted in the calculation: the anisotropic strain εxy = 0, the interface potential P1 = P2 = P0⋅ x and the segregation length l1 = l2 = 0.3 nm, according to Ref. [23]. By comparing the calculated energy for the 1H1E transition with that observed in the PL spectra, we determine the In concentrations to be 0.22 for samples A, B and C, and 0.152 for sample D. This indicates that In atom segregation leads to an upward shift of the transition energy. The simulation results when the effect of In atom segregation is considered are shown in Fig. 5. Comparing Fig. 5(a) with Figs. 3(a) and 4(a), one can see that the sign of the IPOA induced by In atom segregation is opposite to that induced by the anisotropic interface potential and anisotropic strain. As the InGaN thickness increases, the IPOA of the 1H1E and 1L1E transitions decreases, while that of the 2H1E transition does not show any significant change, which is quite close to zero. Figure 5(c) reveals that the IPOA of the 1H1E and 1L1E transitions increases with the In composition. It can be seen from Fig. 5(d) that the IPOA spectrum is mostly made up of contributions from the 1H1E and 1L1E transitions under a small linewidth of 0.01 eV. When considering a large linewidth of 0.2 eV, the ΔM peaks of 1H1E and 1L1E overlap. Due to their closely aligned energies and opposite IPOA signs, the superposition of the peaks results in a significant reduction in the overall peak intensity. It can be seen that the IPOA induced by In atom segregation effect is dominated by 1H1E and 1L1E. Comparing Fig. 5(d) with Fig. 3(d), we note that the calculated IPOA with a line width of 0.2 eV induced by In atom segregation is larger than that induced by the anisotropic interface potential with ΔP = 0.02P1.

    The simulated results indicate that the IPOA induced by anisotropic strain or interface potential is mainly contributed by the transitions of 1H1E, 1L1E and 2H1E, and that induced by In atom segregation effect is dominated by the transitions of 1H1E and 1L1E. The IPOA spectra observed in the experiment are primarily attributed to the 1H1E and 1L1E transitions. This finding is supported by the fact that the position of the peaks in the RDS spectra is closely aligned with that in the PL spectra, which are dominated by 1H1E and 1L1E transitions. Therefore, it can be inferred that the IPOA observed in our samples primarily arises from In atom segregation in InGaN/GaN Qdisks. When using a MoS2/Mo substrate to grow the InGaN Qdisks, the growth temperature is set at 700 °C. In contrast, when employing a Ti/Mo substrate, the growth temperature is reduced to 480 °C. The increase in growth temperature significantly enhances the segregation effect of In atoms, which leads to the larger IPOA in samples A and B.

4.   Conclusion
  • In conclusion, we have investigated the IOPA of InGaN/GaN Qdisks in nanowires grown on MoS2/Mo and Ti/Mo substrates by RDS. It is demonstrated that the IPOA of samples grown on the MoS2/Mo substrate is approximately an order of magnitude larger than that of samples grown on the Ti/Mo substrate. To uncover the origin of the IPOA, we conducted numerical calculations using the six-band k ⋅ p method, incorporating the effects of an anisotropic interface potential, anisotropic strain and indium atom segregation. It is found that the IPOA is primarily driven by the segregation of indium atoms in the InGaN/GaN Qdisks. This study highlights the significant influence of substrate materials on the IPOA of semiconductor heterostructures and in order to effectively control the segregation effect of In atoms, it is preferable to select substrate materials that can achieve high-quality growth at lower temperatures.