Multiferroic materials have been the focus of research in the field of materials science for more than two decades.[1–5] Since the discovery of multiferroicity in thin films of BiFeO3[6] and single crystals of TbMnO3[7] in 2003, a great effort has been devoted to searching for multiferroic materials in various types of compounds. While the majority of multiferroics are inorganic compounds, some progress has also been achieved in organic or inorganic–organic hybrid materials.[8] Especially, a special group of inorganic–organic hybrids, i.e., metal–organic frameworks (MOFs), has been found to exhibit multiferroicity and detectable magnetoelectric (ME) effect.[8–12]
MOFs are usually constructed from inorganic metal nodes connected with organic ligands.[13–15] They are well known for the rich physical and chemical properties due to the diversity of metal ions, organic components, and spatial openness.[16–19] Compared to 3D MOF materials, 2D layered MOFs have an open space between layers, and the size limitations of the organic components between layers are lifted, allowing the accommodation of various organic components. As a result, the layered MOFs may produce a series of unusual physical properties.[20–25] At present, there are still very few ammonium-containing layered MOFs reported so far. In 2018, Chen et al.[26] first synthesized an ammonium-containing layered MOF with a chemical formula of [NH4Cl]2[Ni(HCOO)2(NH3)2] (Ni–MOF), which consists of alternately stacked [Ni(HCOO)2(NH3)2] layers and CsCl-type [(NH3)2(NH4Cl)2] layers. The studies of electric and magnetic properties implied that it could be multiferroic with an antiferromagnetic phase transition near 25 K and a ferroelectric phase transition around 110 K.[26]
In this work, we have performed a systematic investigation on the magnetic, dielectric, pyroelectric properties as well as thermal expansion of this layered Ni–MOF. Our study suggests that the structural transition induces weak ferroelectricity along the c axis and antiferroelectricity in the ab plane. The most interesting finding is a negative thermal expansion (NTE) along the c-axis across the weak ferroelectric phase transition. Moreover, external magnetic fields are able to shift the ferroelectric/antiferroelectric phase transition temperature to a higher temperature, suggesting certain magnetoelectric coupling in the paramagnetic phase.
-
Single-crystal samples of the Ni–MOF were synthesized by the hydrothermal method. The required materials include NiCl2 ⋅ 6H2O (5.0 mmol, 1.189 g), NH4COOH (15.0 mmol, 0.946 g), NH4Cl (15.0 mmol, 0.802 g), N,N-dimethylformamide (25.0 mL) and CH3OH (25.0 mL). The mixed solution was poured into a 100 mL Teflon-lined autoclave and heated in an oven at 80 °C for 4 days. The products are blue rectangular flake crystals (main product) and light green impurity (secondary product). The crystals were washed with ethanol and dried in air, then placed in an inert, oxygen-free environment for storage. The obtained samples were checked with x-ray diffraction (XRD) at room temperature using a diffractometer (Rigaku 2000) with Cu Kα radiation (λ = 1.54056 Å).
The magnetic properties were measured in a Quantum Design magnetic property measurement system (MPMS). The specific heat in the temperature range of 2 K to 200 K was measured in a Quantum Design physical property measurement system (PPMS). The dielectric permittivity and pyroelectric current were measured by using a home-made probe in the PPMS. Silver paste was applied to the upper and lower surfaces of the crystals as electrodes. The dielectric permittivity was measured by using a Keithley 4980A LCR meter. For the measurement of pyroelectric current, the samples were firstly cooled under a poling electric field (3.3 kV/cm) from 150 K to 80 K. Then the poling electric field was removed and the electrodes were short-circuited for 30 min to release space charges. Finally, the samples were heated at a rate of 2 K/min while the pyroelectric current (I) was measured using a Keithley 6517B electrometer. The electric polarization was obtained by integrating the pyroelectric current with time. The thermal expansion of the crystals was tested by a capacitance method[27] in an Oxford Instruments superconducting magnet. The capacitance dilatometer was calibrated by using a 99.999% pure copper rod.
-
Figure 1(a) illustrates the crystalline structure of the Ni–MOF at room temperature. It is an orthorhombic structure with the polar space group Aba2.[26] The key structural feature comprises a [Ni(HCOO)2(NH3)2] perovskite layer and a CsCl-type [(NH3)2(NH4Cl)2] layer, with the two interleaved layers arranged in an ABAB stacking pattern within each unit cell. The Ni(HCOO)2(NH3)2 layer consists of Ni2+ ions linked by equatorial anti-anti HCOO− bridges and further coordinated by two axial NH3, as depicted in Fig. 1(b). Notably, the Ni–MOF features a metal–organic layer interspersed with inorganic components, distinguishing it from most layered organic-inorganic hybrids. The XRD pattern of a single-crystal sample at room temperature is shown in Fig. 1(c), which demonstrates that the crystal grows naturally in a layer-by-layer manner along the [001] direction and no impurity phase is detected. The inset shows a photograph of the grown crystal as a rectangular plate, with the c direction perpendicular to the rectangular plane.
The temperature dependence of magnetization along the c-axis measured with both the zero-field-cooling (ZFC) and field-cooling (FC) modes in 2000 Oe is plotted in Fig. 2(a). A paramagnetic to antiferromagnetic (AFM) transition, evidenced by a pronounced peak, was observed around TN ∼ 36 K, followed by a gradual rise below ∼ 10 K. The ZFC and FC curves are almost identical, suggesting a long-range magnetic order along the c-axis. We note that the M–T behavior is similar to that reported in Ref. [26], where TN is defined as the maximum point of dM/dT ∼ 25 K. Not the way we define it, so the temperature is different. The M–H curves measured along the c-axis exhibit a small hysteresis at temperatures below TN, as shown in Fig. 2(b). The almost linear dependence of magnetization on field is consistent with AFM ordering, but the magnetic hysteresis with a small remanence indicates that there is a weak ferromagnetic component. This could be due to uncompensated magnetization of canted AFM order. As shown in Fig. 2(c), the temperature dependence of magnetization for H⊥c-axis exhibits a peak at TN ∼ 32 K, which is slightly lower than that along the c-axis. Below 20 K, the magnetization keeps rising with decreasing temperature. The M–H curves for H⊥c-axis are similar to those for H||c-axis, also suggesting canted AFM order.
Temperature dependence of heat capacity was measured to obtain further insights into the phase transitions in the Ni–MOF. As seen in Fig. 3, the heat capacity exhibits three peaks around 25 K, 100 K, and 110 K, respectively, indicating three separate phase transitions. The peak at ∼ 25 K corresponds to the AFM magnetic phase transition, and the peaks at 100 and 110 K correspond to two structural phase transitions.
Figure 4(a) illustrates the dielectric permittivity along the c-axis as a function of temperature in the range of 2–150 K with both cooling and warming processes. During warming, εc increases rapidly above ∼ 100 K and reaches a maximum around 120 K, which is likely due to the successive structural phase transitions. The hysteresis between the warming and cooling processes suggests the nature of the first-order phase transitions. In contrast, the dielectric permittivity perpendicular to the c-axis as a function of temperature exhibits multiple peaks/kinks, as shown in Fig. 4(b). The small hump around 30 K could be due to the magnetic transition, while the peaks around 84 K and 107 K are likely related to the structural phase transitions. Moreover, the relative dielectric permittivity in the ab-plane is significantly lower than that along the c-axis. When a magnetic field (9 T) is applied along the c-axis, the dielectric permittivity εc changes slightly. In contrast, when a magnetic field (9 T) is applied in the ab plane, the dielectric permittivity εab changes more clearly. The structural phase transition temperature shifts to a higher temperature in 9 T.
To reveal the nature of the structural phase transitions, we measured the pyroelectric current with temperature after poling the sample in an electric field E||c axis or E⊥c axis. As shown in Fig. 5(a), a sharp peak at 104 K followed by a broad peak around 113 K in pyroelectric current was observed for E||c-axis. The obtained electric polarization along the c axis is ∼ 0.5 nC/cm2 (Fig. 5(c)), three orders less than that of conventional ferroelectrics. This small electric polarization indicates that the structural phase transitions induce weak ferroelectricity along the c-axis. For E⊥c axis, a very weak peak is barely detected in the pyroelectric current around 103 K and the electric polarization is only 0.02 nC/cm2, as shown in Figs. 5(b) and 5(d), respectively. It is more likely that the tiny electric polarization for E⊥c axis is due to antiferroelectric order. Based on the pyroelectric current results, it is concluded that the structural transitions induce weak ferroelectricity along the c-axis and antiferroelectricity in the ab plane.
To further investigate the structural phase transitions, we measured thermal expansion using a capacitance method. The linear thermal expansion along the c-axis is presented in Fig. 6(a). The length of the crystal increases with temperature till 100 K, and then decreases between 100 K and 107 K. As a result, an NTE (∼ 452 ppm) is observed between two structural phase transitions (100–110 K). NTE has been widely observed in a number of inorganic materials,[28–31] and its mechanism could be related to a variety of physical properties such as ferroelectricity, magnetism, and superconductivity.[32–35] Due to the porous framework and large-scale flexibility, MOF compounds also display NTE.[36–38] The attributed mechanisms include electronic and magnetic transitions, transverse atomic and molecular vibrations, and so on. In the Ni–MOF, the [Ni(HCOO)2(NH3)2] chalcogenide layer and the CsCl-type [(NH3)2(NH4Cl)2] layer share NH3 groups axially coordinated to Ni2+, forming N–H–Cl hydrogen bonds. The weak ferroelectricity along the c-axis could be due to the hydrogen bond ordering. When the temperature is above the structural transition temperature (100 K), the hydrogen bonds start to become disordered until the second structural transition temperature. During this process, the interlayer hydrogen bonding length may shrink with increasing temperature, causing an anomalous negative thermal expansion along the c-axis. When a magnetic field (9 T) is applied along the c-axis, the magnitude of the negative thermal expansion decreases to ∼ 417 ppm, and the phase transition temperature shifts to a higher temperature by 1.5 K, as shown in Fig. 6(c). In contrast, as seen in Fig. 6(b), the thermal expansion in the ab plane does not show a negative thermal expansion. The two kink points are consistent with two structural transitions. Additionally, the phase transition shifts to a higher temperature by ∼ 0.7 K under 9 T magnetic field (Fig. 6(d)). These results suggest that external magnetic fields would stabilize the ordering of hydrogen bonds through magnetoelastic coupling of Ni ions so that the order-disorder transition shifts to a higher temperature. The influence of the magnetic field on the structural phase transitions as evidenced in the shift of dielectric permittivity and thermal expansion implies the ME coupling in the paramagnetic state of the Ni–MOF.
-
In conclusion, we have investigated the magnetic, dielectric, pyroelectric, and thermal expansion properties of the layered perovskite Ni–MOF. The results reveal a canted AFM transition at ∼ 36 K, and two successive structural phase transitions around 100 K and 110 K. Moreover, the structural transitions are found to induce weak ferroelectricity along the c-axis and antiferroelectricity in the ab plane. A negative thermal expansion of ∼ 452 ppm along the c-axis appears between the two structural phase transitions, which is ascribed to the shrinkage of interlayer hydrogen bonding length during the order-disorder process. The shift of the structural phase transition temperature under a magnetic field implies the ME coupling even in the paramagnetic state.