2025 Volume 34 Issue 7
Article Contents

Xuyang Li, Bin Liu, Xianwen Liu, Shuo Zhang, Congyang Wen, Jin Zhang, Haifeng Liang, Guangcai Yuan, Jianshe Xue, Zhinong Yu. Performance enhancement of IGZO thin-film transistors via ultra-thin HfO2 and the implementation of logic device functionality[J]. Chinese Physics B, 2025, 34(7): 076101. doi: 10.1088/1674-1056/adcb22
Citation: Xuyang Li, Bin Liu, Xianwen Liu, Shuo Zhang, Congyang Wen, Jin Zhang, Haifeng Liang, Guangcai Yuan, Jianshe Xue, Zhinong Yu. Performance enhancement of IGZO thin-film transistors via ultra-thin HfO2 and the implementation of logic device functionality[J]. Chinese Physics B, 2025, 34(7): 076101. doi: 10.1088/1674-1056/adcb22

Performance enhancement of IGZO thin-film transistors via ultra-thin HfO2 and the implementation of logic device functionality

  • Received Date: 28/02/2025
    Accepted Date: 25/03/2025
    Available Online: 01/07/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(9)  /  Tables(2)

Article Metrics

Article views(718) PDF downloads(2) Cited by(0)

Access History

Performance enhancement of IGZO thin-film transistors via ultra-thin HfO2 and the implementation of logic device functionality

Abstract: The enhancement of mobility has always been a research focus in the field of thin-film transistors (TFTs). In this paper, we report a method using ultra-thin HfO2 to improve the electrical performance of indium gallium zinc oxide (IGZO) TFTs. HfO2 not only repairs the surface morphology of the active layer, but also increases the carrier concentration. When the thickness of the HfO2 film was 3 nm, the mobility of the device was doubled (14.9 cm2·V−1·s−1 → 29.6 cm2·V−1·s−1), and the device exhibited excellent logic device performance. This paper provides a simple and effective method to enhance the electrical performance of IGZO TFTs, offering new ideas and experimental foundation for research into high-performance metal oxide (MO) TFTs.

1.   Introduction
  • Metal oxide (MO) thin-film transistors (TFTs) are widely used in display devices due to their high visible-light transmittance, good stability and excellent electrical performance.[1–3] Since they were first proposed as the mainstream MO TFTs, indium gallium zinc oxide (IGZO) TFTs have attracted extensive attention.[4–9] Characterized by advantages, such as low off-current, high mobility and wide band gap, IGZO TFTs have been extensively applied in display drivers, electronic skins and detectors.[10–13]

    With the rapid development of the display industry, the demand for high-refresh-rate and high-definition displays has driven continuous improvement in the mobility of MO TFTs.[14,15] Enhancing the electrical performance of devices has always been a research focus in the field of MO TFTs. For example, using a dual-active-layer structure can boost MO TFT mobility. Two different active-layer materials will increase the carrier concentration and form a two-dimensional electron gas at the heterojunction interface, thus improving the electrical performance and stability of the devices.[16–20] However, requiring two types of semiconductor materials, this method raises device manufacturing costs. Some studies have treated the active layer with plasma to adjust the surface morphology of the thin film and the oxygen vacancy concentration in the active layer, thus enhancing the device electrical performance.[21–25] However, this method requires precise control of the plasma gas process, increasing the complexity of device manufacturing. Some studies have improved the stability of devices by controlling the annealing atmosphere (such as introducing argon or hydrogen during annealing).[26,27] However, the improvement effect of this method is limited. Recently, some studies on metal oxide capping layers modifying the active layer have gained attention, such as using alumina, calcium oxide, etc, as metal oxide capping layers to modify the active layer.[28–30] Typically, the metal oxide modification layer is placed above the active layer. This method not only prevents the active layer from contacting environmental water vapor, enhancing device environmental stability, but also increases carrier concentration within the active layer, significantly improving device electrical performance.

    In this paper, we report on the impact of an ultra-thin hafnium dioxide (HfO2) modification layer on the performance of IGZO TFTs. We deposited HfO2 thin films of different thicknesses on the active layer of TFTs as a modification layer. We then analyzed the effect of the thickness of the modification layer on the performance of TFTs. The experimental results show that while HfO2 can enhance device performance, an excessively thick modification layer is detrimental. We explained this experimental phenomenon by a combination of test analysis and technology computer-aided design (TCAD) simulation. On the one hand, the HfO2 modification layer can make the surface of the active layer smoother, improving the carrier transport efficiency. On the other hand, a suitably thick HfO2 modification layer increases the carrier concentration within the active layer. However, an overly thick modification layer introduces too many acceptor defect states and increases the difficulty of current tunneling between the active layer and the electrode. This work provides a new theoretical basis and experimental approach for the realization of high-performance TFTs. We also fabricated the optimized TFTs into a single-device inverter, demonstrating their potential for application in logic circuits.

2.   Experiment details
  • All TFT devices were fabricated using a bottom-gate and top-contact structure, and the fabrication process is shown in Fig. 1. We used heavily doped n-type thermal oxide silicon as the substrate, as shown in Fig. 1(a), where polysilicon was used as the gate electrode and silicon dioxide with a thickness of 100 nm was used as the dielectric layer. The cleaned substrate was placed into a vacuum chamber and sputtered using a shadow mask, as shown in Fig. 1(b). A 20 nm thick IGZO film was sputtered as the active layer, with a sputtering power of 50 W and a flow rate of argon and oxygen of 40 sccm:5 sccm. The base vacuum was set at 5 × 10−4 Pa and the sputtering vacuum was set at 0.8 Pa. The metal element ratio in IGZO target materials is In:Ga: Zn = 1:1:1. After sputtering the IGZO film, the target source was switched, and HfO2 films with thicknesses of 0 nm, 1 nm, 3 nm, 5 nm and 7 nm were sputtered as the modification layers, with a sputtering power of 45 W and a flow rate of argon and oxygen of 40 sccm:20 sccm. The base vacuum was set at 5 × 10−4 Pa and the sputtering vacuum was set at 0.8 Pa. The sputtered samples were then annealed in a furnace at 300 °C for 1 hour, as shown in Fig. 1(c). After the samples cooled down, we used thermal evaporation to deposit aluminum metal with a thickness of 100 nm as the source electrode and drain electrode. During evaporation, we used a shadow mask to pattern the electrodes, resulting in a channel length of 100 μm and a width of 1000 μm, as shown in Fig. 1(d).

    The electrical performance of the devices was tested using a Keithley 2636B in a room-temperature dark environment. The surface morphology of the active layer was observed using an atomic force microscope (AFM, Bruker Dimension ICON) to study the quality of the film. The chemical state of the films was analyzed using x-ray photoelectron spectroscopy (XPS, Thermo Scientific K-Alpha). The changes in the carrier concentration within the active layer were analyzed using TCAD simulation.

3.   Results and discussion
  • We first conducted atomic force microscopy (AFM) measurements on the sample surface within a 2 μm × 2 μm scan area, and the results are presented in Figs. 2(a)–2(e). The numerical values labeled in the figures correspond to the HfO2 film thicknesses, and this labeling convention is maintained throughout subsequent figures. Based on the AFM images of the samples, we were able to calculate the root mean square (RMS) value of the surface roughness of the samples, as shown in Fig. 2(f). As can be clearly seen from Fig. 2(f), the active layer modified with HfO2 has a lower surface roughness. We propose that during HfO2 sputtering, the plasma generated in the vacuum chamber may effectively repair the IGZO surface defects. Consequently, compared with unmodified films, the RMS value of the active layer with 1 nm HfO2 deposition decreases significantly. Moreover, as the thickness of HfO2 increased, the continuity of the HfO2 film was enhanced, further smoothing the sample surface. After plasma modification, the smooth interlayer interface helps to reduce the interface trapping effect and promote charge injection and transport,[31,32] which is beneficial to improve the electrical performance of the devices.

    We fabricated all samples into TFT devices and evaluated their output characteristics, and the results are shown in Figs. 3(a)–3(e). All samples demonstrated n-type TFT performance with clear pinch-off voltages. At low source–drain voltage (VDS), the source–drain current (IDS) rose linearly with VDS, indicating good ohmic contact between the electrodes and the active layer.[33–35] At high VDS, IDS showed a significant saturation phenomenon. The output characteristic curves of all samples at a gate voltage (VGS) of 40 V are shown in Fig. 3(f), and we extracted the linear part of the curves. We compared the IDS values of the samples when VDS was 10 V. We found that the IDS value of the sample was the highest when the thickness of HfO2 was 3 nm; when the thicknesses of HfO2 were 5 nm and 7 nm, the IDS values of the samples decreased significantly.

    We further evaluated the transfer characteristics of the devices at a fixed VDS of 10 V, as depicted in Fig. 4. According to the transfer characteristic curves, all the samples exhibited switching characteristics, with a switching ratio greater than 105. Notably, at VGS = 40 V, the IDS variation trend aligned with that in Fig. 3(f). Based on the transfer characteristic curves, we were able to calculate the electrical parameters of the devices such as the field-effect mobility (μFE), threshold voltage (Vth), subthreshold swing (SS) and switching ratio (Ion/Ioff). The electrical parameters of the samples are shown in Table 1.

    As shown in Table 1, the mobility of the samples first rose with the increase in HfO2 thickness. However, when the thickness of HfO2 exceeded 3 nm, the mobility of the samples decreased with the increase in HfO2 thickness. We attribute this to HfO2 altering the oxygen vacancy concentration in the IGZO film, as depicted in Fig. 5. The Hf–O bond strength (802 kJ/mol) far exceeds that of the In–O (346 kJ/mol), Ga–O (374 kJ/mol) and Zn–O (284 kJ/mol) bonds.[36–38] During annealing, some weak metal-oxygen bonds in the IGZO film broke, creating oxygen vacancies, while the released oxygen combined with hafnium to form stable Hf–O bonds. As the thickness of HfO2 increased, the oxygen vacancy concentration in the IGZO film continuously increased. The increase in oxygen vacancy concentration increases the electron concentration in the channel.[28,39] According to the percolation model, the mobility of amorphous oxide semiconductors will increase with the increase in carrier concentration.[40,41] This explains why the mobility of the devices increased with the increase in HfO2 thickness when the thickness of HfO2 was less than or equal to 3 nm. However, as the oxygen vacancy concentration further increased, more band tail states were introduced in the active layer.[42] These defect states act as scattering centers, increasing carrier scattering during transport and capturing carriers, thus reducing mobility. The subthreshold swing increase with HfO2 thickness also indicates rising defect state concentration. The difficulty of electron tunneling between the active layer and the electrode also increased with the increase in HfO2 thickness, and the increase in threshold voltage with the increase in HfO2 thickness confirmed this point. In other words, the HfO2 film exhibited increasingly stronger insulating properties as its thickness increased. This also had a negative impact on the mobility of the device. When the thickness of HfO2 was 7 nm, the threshold voltage had already reached 6.68 V and the switching ratio was only in the order of 105.

    To verify the above analysis, all samples were tested by x-ray photoelectron spectroscopy (XPS). The O 1s spectra of all samples are shown in Figs. 6(a)–6(e). By deconvoluting the O 1s spectra with a Gaussian function, three sub-peaks with binding energies at 530.3 ± 0.1 eV, 531.9 ± 0.1 eV and 532.8 ± 0.1 eV were obtained. These three sub-peaks correspond to oxygen bonded to metal (M–O–M), oxygen vacancies (M–VO) and hydroxyl groups (M–OH).[25] The variation trend of the area ratios of the three sub-peaks is shown in Fig. 6(f). When the thickness of HfO2 was less than or equal to 3 nm, the oxygen vacancy content increased stepwise. This trend was consistent with the previous analysis, indicating that the deposited HfO2 introduced extra oxygen vacancies into IGZO. However, when the thickness of HfO2 exceeded 3 nm, the concentration of oxygen vacancies did not increase significantly but rather showed a downward trend, which was inconsistent with the previous analysis trend. This is because XPS tests the surface of the samples. The information collected by the O 1s spectrum is approximately a 10 nm thick film. Since Hf has a higher affinity for oxygen, although the concentration of oxygen vacancies in the IGZO film increases, Hf also combines with oxygen from the air to form metal-oxygen bonds. That is, when the thickness of HfO2 exceeds 3 nm, although the concentration of oxygen vacancies in the IGZO film increases stepwise, the concentration of oxygen vacancies in HfO2 is relatively low due to the higher proportion of metal-oxygen bonds in HfO2. As a result, statistically, the concentration of oxygen vacancies appears to decrease rather than increase. This can be proved by the increasing content of metal-oxygen bonds.

    To verify the effect of HfO2 thickness on the electron concentration in the active layer, we conducted TCAD simulations, as shown in Fig. 7. Figure 7(a) shows the simulated cross-sectional view of the IGZO TFTs. The active layer parameters were set based on Fung et al.’s work,[41] including the effective density-of-states (DOS) in the conduction and valence bands, electron affinity, etc. The specific parameters are given in Table 2. Figure 7(b) shows the local enlargement of the active layer and the modifying layer, where the thickness of HfO2 was set at 0 nm, 1 nm, 3 nm, 5 nm and 7 nm, respectively. Figure 7(c) illustrates the device structure mesh division. The electrode region has a relatively sparse mesh for rougher calculations, while the active and modifying layers have a denser mesh for more detailed calculations. Figure 7(d) shows the electron concentration distribution map in the device after setting VGS at 40 V and VDS at 10 V and running the calculation.

    The electron concentration distribution maps allow quantitative analysis of how electron concentration varies with film depth, as depicted in Figs. 8(a)–8(e). By integrating these data, the electron concentration of different samples can be quantitatively determined, as shown in Fig. 8(f). Figure 8(f) reveals that the electron concentration in IGZO peaks at a HfO2 thickness of 3 nm is consistent with prior analysis. This proves that when the thickness of HfO2 is less than or equal to 3 nm, HfO2 will enhance the carrier concentration in the active layer, thereby increasing the mobility of the device. However, when the thickness of HfO2 exceeds 3 nm, not only will the additional oxygen vacancies capture carriers, leading to a decrease in electron concentration, but the overly thick HfO2 film also reduces the injection efficiency of source charge due to its strong insulating properties.

    In summary, when the thickness of HfO2 is 3 nm, the overall performance of the device is optimal. We fabricated a single-device inverter using the sample with a modifying layer thickness of 3 nm to test its feasibility for application in logic circuits.

    As shown in Fig. 9(a), we fabricated an inverter using the IGZO TFT with an HfO2 thickness of 3 nm. Vin is the input voltage terminal, Vout is the output voltage terminal and VDD is the operating voltage. We tested its voltage transfer characteristics by setting VDD at 1 V and 5 V, respectively, and the results are shown in Fig. 9(b). When Vin is 0 V, Vout is approximately equal to VDD, and Vout is at a high logic level; when Vin is equal to VDD, Vout is approximately equal to 0 V, and Vout is at a low logic level. Thus, the device meets the inverter’s logic output requirements. The gain can be obtained by differentiating the voltage transfer characteristic curve. As shown in Fig. 9(c), the gain of the device is much greater than 1, indicating its potential to drive complex logic circuits.[43] We also assessed the inverter’s dynamic response, as shown in Fig. 9(d), and it exhibited a good dynamic response under a 1 Hz AC square wave. In summary, the HfO2-optimized IGZO TFT has great potential for application in logic circuits.

4.   Conclusion
  • In this paper, we introduced a method to modify the active layer of IGZO TFTs using ultra-thin HfO2 films. We found that the comprehensive performance of IGZO TFTs was optimal when the thickness of the HfO2 film was 3 nm. Compared with the unmodified control samples, the mobility of the TFTs modified by the HfO2 film was doubled (14.9 cm2·V−1·s−1 → 29.6 cm2·V−1·s−1). This improvement can be attributed to two factors. First, the dense oxide film can heal the active layer’s surface morphology, reducing roughness and enhancing carrier transport efficiency. Second, the strong Hf–O bonds can introduce more oxygen vacancies into the active layer. An appropriate concentration of oxygen vacancies increases the carrier concentration within the active layer, thereby enhancing device mobility. In addition, we fabricated the optimized device into a single-device inverter, which exhibited good performance and demonstrated the application potential of TFTs in logic circuits. This paper provides a new experimental idea and theoretical foundation for the fabrication of high-performance TFTs.

Figure (9)  Table (2) Reference (43)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return