2025 Volume 34 Issue 6
Article Contents

Yang-Kun Zhang, Yu-Chen Wang, Wei Yang, Dong-Xia Shi, Luo-Jun Du, Guang-Yu Zhang. Two-step growth of 4-inch multilayer MoS2 wafers[J]. Chinese Physics B, 2025, 34(6): 068103. doi: 10.1088/1674-1056/adce9f
Citation: Yang-Kun Zhang, Yu-Chen Wang, Wei Yang, Dong-Xia Shi, Luo-Jun Du, Guang-Yu Zhang. Two-step growth of 4-inch multilayer MoS2 wafers[J]. Chinese Physics B, 2025, 34(6): 068103. doi: 10.1088/1674-1056/adce9f

Two-step growth of 4-inch multilayer MoS2 wafers

  • Received Date: 07/03/2025
    Accepted Date: 18/04/2025
    Available Online: 01/06/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(4)

Article Metrics

Article views(795) PDF downloads(4) Cited by(0)

Access History

Two-step growth of 4-inch multilayer MoS2 wafers

Abstract: Molybdenum disulfide (MoS2) is an emerging two-dimensional (2D) semiconductor and has great potential for high-end applications beyond the traditional silicon-based electronics. Compared to the monolayers, multilayer MoS2 has improved electron mobility and current density, and therefore provides a more promising platform in terms of thin-film transistors, flexible electronic devices, etc. However, the synthesis of large-area, high-quality multilayer MoS2 films with controlled layer number remains a challenge. Here, we develop a two-step oxygen-assisted chemical vapor deposition (OA-CVD) methodology for the synthesis of 4-inch MoS2 films from monolayer to trilayer on sapphire substrates. The influence of critical growth parameters on the growth of multilayer MoS2 is systematically explored, such as the evaporation temperature of MoO3 and the flow rate of O2. Flexible field-effect transistor (FET) devices fabricated from bilayer/trilayer MoS2 show substantial improvements in mobility compared with flexible FETs based on monolayer films.

1.   Introduction
  • Molybdenum disulfide (MoS2) has been considered as one of the most promising two-dimensional (2D) semiconductor candidates for extending Moore’s law beyond traditional silicon-based electronics[1] and developing advanced technological applications in nanoelectronics and optoelectronics,[2–5] owing to its high mobility, excellent gate controllability, high on/off current ratio, excellent thermal stability, low dielectric constant and high mechanical strength.[6–9] To realize its full potential and real-world application, the controllable synthesis of large-area, high-quality MoS2 films is highly desired. Since the first production of monolayer MoS2 in 2012,[10] notable progress has been witnessed in the synthesis of large-scale monolayer MoS2 over the past decade. Until now, high-quality monolayer MoS2 wafers up to 12-inch have been synthesized by various growth approaches,[11,12] including chemical vapor deposition (CVD),[12–16] metal-organic CVD (MOCVD),[17,18] molecular beam epitaxy (MBE),[19] and atomic layer deposition (ALD).[20,21] However, owing to several fundamental limitations,[22,23] (e.g., phonon-limited mobility, large Schottky barrier height, and Fermi-level pinning), further improvement of the electronic quality of monolayer MoS2 faces great challenges.

    A promising alternative is the multilayer MoS2, such as bilayer and trilayer, as both quantum transport simulations and experiments have consistently shown the enhanced electron mobilities and current densities.[24–27] Although some attempts have been made to grow multilayer MoS2,[28] it currently remains a significant challenge to produce large-scale bilayer/trilayer MoS2 film with control over yield, orientation and uniformity. In addition, previous studies typically adopted a one-step direct synthesis strategy,[29,30] which limited the systematic investigation on the effect of different growth parameters on the growth of multilayer MoS2.

    Here, we design a two-step oxygen-assisted chemical vapor deposition (OA-CVD) methodology to synthesize 4-inch MoS2 films from monolayer to trilayer on sapphire substrates. Compared with the previous one-step synthesis method, our two-step OA-CVD strategy can precisely control the growth of each layer independently, thus facilitating the possibility to investigate the growth parameters on the growth of multilayer MoS2. The influence of critical synthesis parameters, such as the evaporation temperature of MoO3 (TMo) and the oxygen flow rate (FO2), on the growth of multilayer MoS2 is systematically explored. Flexible field-effect transistor (FET) devices fabricated from bilayer (trilayer) MoS2 show 45.5% (109.1%) improvements in average mobility compared with flexible FETs based on monolayer films.

2.   Methods
  • Single-sided polished C-plane (0001) sapphire substrates with a miscut angle of ∼ 0.2° toward the M-axis were purchased from Cryscore Optoelectronic Limited. Then, the sapphire substrates were annealed to reconstitute the surface at ∼ 1000 °C for 4 h in the presence of oxygen. The growth of multilayer MoS2 was achieved in a custom-designed three-temperature zone CVD system with multisource design. Typically, 25 g and 12 g sulfur powder (Shanghai Aladdin Biochemical Technology, 99.999%) for synthesizing monolayer and multilayer MoS2 were placed in the center mini-tube flowed with 40 sccm Ar. MoO3 powder (Alfa Aesar, 99.999%) was pressed into thin flakes by a hydraulic press and divided into three equal parts, which were individually placed in three quartz tubes with equilateral triangular distribution flowed with Ar/O2 (40/2 sccm), and the other three empty tubes were also flowed with Ar/O2 (40/2 sccm). During the growth, the sulfur powder was heated to 180 °C and 160 °C for synthesizing monolayer and multilayer MoS2 in the temperature zone of sulfur by a heating mantle. The MoO3 flacks were heated to 580 °C and 610 °C for synthesizing monolayer and multilayer MoS2 in the temperature zone of MoO3, and the sapphire substrate was heated to 930 °C. In addition, the pressure of CVD system was kept below 1 torr during the growth process and then cooled naturally to room temperature in the Ar stream after the growth. The growth durations of monolayer, bilayer and trilayer MoS2 films were 40 min, 15 min, and 25 min, respectively.

    In addition, the annular STEM and SAED characterizations were performed by an aberration-corrected STEM (JEM-ARM200F) at 200 kV. AFM imaging was carried out by Asylum Research Cypher S in tapping mode, using the tip AC240TS-R3 (Oxford Instruments). Raman and photoluminescence spectra were collected with a HORIBA spectrometer (LabRAM HR Evolution) in a confocal backscattering configuration (confocal pinhole of 100 μm) at room temperature. A solid-state laser at 532 nm was focused onto the samples along the z direction by a ×100 objective with a spot size less than 1.5 μm.

    Furthermore, to fabricate flexible back-gate FET, Ti (3 nm)/Au (10 nm)/Ti (2 nm) was patterned and deposited on PET substrate as local back gate. Next, 20 nm aluminum oxide (Al2O3) was applied as dielectric insulator using atomic layer deposition (ALD) at a temperature of 120 °C, utilizing water (H2O) and trimethyl aluminum as precursors. Subsequently, the MoS2 films were etched off from sapphire substrates in KOH solution (1 mol/L) at 110 °C and transferred onto the Al2O3 layer assisted by deionized water. The channel area was then defined using lithography, followed by reactive ion etching (RIE) to shape it. Finally, contact electrodes were defined by lithography and Au (10 nm)/Ti (3 nm)/Au (30 nm) were finally deposited. The entire patterning procedure was carried out using the direct-write laser lithography (DWL 66+) and developed using TMAH developer (AZ 300MIF). Metal electrodes were deposited using a custom-built electron beam deposition system and then subjected to the lift-off process.

3.   Results and discussion
  • Figure 1(a) illustrates the process for growing multilayer MoS2 via a two-step OA-CVD methodology. Monolayer MoS2 films are first grown on 4-inch C-plane (0001) sapphire with 0.2° miscut angle toward the M-axis (〈101¯0〉) by a self-designed 4-inch OA-CVD system with sulfur powder and MoO3 as the precursor. Then, the as-grown monolayer MoS2 is placed back into the CVD system and used as the substrate to achieve the growth of bilayer MoS2 films. Furthermore, the as-grown bilayer MoS2 is placed back into the CVD system and used as the substrate to achieve the growth of trilayer MoS2 films. We highlight that owing to the higher nucleation barrier of multilayer MoS2, the growth parameters of monolayer MoS2 and multilayer MoS2 are usually quite different.[31–34] Therefore, the previous one-step growth method, which is difficult to realize the compatibility and fast switching of growth parameters between monolayer and multilayer MoS2, makes large-area uniform multilayer MoS2 growth challenging. By contrast, the two-step OA-CVD strategy can precisely control the growth of each layer independently, thus facilitating the possibility to control the growth of multilayer MoS2. It is noteworthy that to avoid the etching of monolayer MoS2 by oxygen and high temperature during the early stages of the second growth, oxygen would be supplied after ensuring that the sulfur source in the quartz tubes is excessive.

    Figures 1(b)–1(d) show the photographs of the as grown 4-inch monolayer, bilayer and trilayer MoS2 wafers, respectively. The homogeneity in color illustrates the uniformity of these MoS2 films. Figures 1(e)–1(g) show typical optical microscopy images of these as-grown MoS2 film wafers, indicating full coverage and very clean surfaces (please refer to Fig. S1 for more optical images). Note that for trilayer MoS2 continuous films, there are certain additional small quadrilayer MoS2 domains and their coverage is less than ∼ 20%. The layer numbers are further confirmed by atomic force microscopy (AFM) measurements after we scrape off the MoS2 films with a tweezer [Figs. 1(h)–1(j)]. The measured thickness of ∼ 0.7 nm, ∼ 1.2 nm, and ∼ 1.8 nm is in good harmony with thickness of monolayer, bilayer, and trilayer MoS2, receptively.

    As MoS2 would have layer-dependent properties, we characterized the optical properties of the as-grown monolayer, bilayer and trilayer MoS2 films. Figure 2(a) demonstrates the corresponding Raman spectra. Two prominent peaks can be seen, originating from the in-plane E2g and out-of-plane A1g modes at the Brillouin-zone center of the monolayer constituent. The peak frequency difference between the E2g and A1g vibrational modes is ∼ 21 cm−1 for monolayer MoS2, while it increases to ∼ 24 cm−1 (∼ 25 cm−1) for bilayer (trilayer) MoS2. Besides, the photoluminescence (PL) spectra of monolayer, bilayer, and trilayer MoS2 films are shown in Fig. 2(b). A strong A exciton emission peak at ∼ 1.88 eV can be observed for monolayer MoS2. In contrast, the A exciton emission intensities are greatly suppressed and the peak position is red-shifted in bilayer and trilayer MoS2. This is due to the transition from the direct bandgap of monolayer MoS2 to the indirect ones of bilayer/trilayer MoS2.[7,8] It is worth noting that the sharp peak at ∼ 1.79 eV comes from the sapphire substrate.

    To clarify the stacking order in these multilayer MoS2 wafers, we perform atomic structure characterization using selected transmission electron microscopy (STEM). The STEM results show that the as-grown bilayer MoS2 exhibits two stacking orders: AA stacking (3R phase) and AB stacking (2H phase), with the corresponding atomic configurations shown in Fig. 2(c). Note that the AA-stacked bilayer MoS2, which breaks both the inversion and out-of-plane mirror symmetries, belongs to exotic 2D sliding ferroelectric semiconductor and promises the prospect of emerging technological applications like brain-inspired in-memory computing, neuromorphic computing.[35] Figures 2(d) and 2(e) show, respectively, the STEM images of typical AA- and AB-stacked bilayer MoS2. For AA-stacked bilayer MoS2, atoms are located not only at the corners of the honeycomb lattice, but also at its center. By contrast, atoms are located only at the corners of the hexagonal lattice for AB-stacked bilayer MoS2. Figure 2(f) displays the selected-area electron diffraction (SAED) pattern of the as-grown bilayer MoS2, which shows only one set of hexagonal diffraction spots. This suggests the high crystalline quality of the as-grown MoS2 and excellent lattice alignments. We also characterized the trilayer MoS2 samples, where AAB/ABB and ABA stacking configurations can be observed (Fig. S3).

    As mentioned above, the two-step OA-CVD growth strategy can precisely control the growth of each layer independently, thus facilitating the possibility to investigate the synthesis parameters on the growth of multilayer MoS2. Here, we respectively investigate the influences of the evaporation temperature of MoO3 (TMo), the oxygen flow rate (FO2), the growth temperature (T) and the growth time (t) on the growth of multilayer MoS2. As shown in Figs. 3(a)–3(c), we increase the TMo from 590 °C to 620 °C while keeping other growth parameters unchanged. Under a low TMo, such as 590 °C, the bilayer MoS2 domains have low nucleation density and therefore cannot be seamlessly stitched into a film [Fig. 3(a)]. Increasing the TMo, the enhanced nucleation density would result in the formation of a seamlessly stitched continuous bilayer MoS2 film [Fig. 3(b)]. However, when the TMo is too high, there would be lots of MoOx impurities on bilayer MoS2 that have not been fully sulfurized [Fig. 3(c)].

    The effect of the oxygen flow rate (FO2) on the growth of multilayer MoS2 is studied by changing FO2 from 8 sccm to 14 sccm while keeping other growth parameters unchanged, as shown in Figs. 3(d)–3(f). The oxygen plays two roles: increasing the growth rate and etching.[36] When FO2 is low, the low growth rate makes it difficult to obtain a seamlessly stitched continuous bilayer MoS2 film. Indeed, many holes that have not been stitched together can be observed when FO2 is only 8 sccm [Fig. 3(d)]. In addition, there are also many trilayer domains owing to the low etching rate. Increasing FO2, the synergistic effect of enhanced growth and etching rates results in the formation of a continuous bilayer MoS2 film essentially free of trilayer grains [Fig. 3(e)]. However, when FO2 is too high, the etching process dominates and thus only discrete bilayer MoS2 domains can be obtained [Fig. 3(f)].

    The effect of the growth temperature on the growth of multilayer MoS2 is studied by changing the growth temperature from 900 °C to 960 °C while keeping other growth parameters unchanged, as shown in Figs. 3(g)–3(i). When the growth temperature is low (900 °C), enhanced adsorption of the precursors on sapphire substrates and weaker oxygen etching promote nucleation density, resulting in lots of small trilayer grains on bilayer MoS2 [Fig. 3(g)]. As temperature increases (930 °C), the enhanced diffusion capacity of precursor and etching effect of oxygen cause a decline in nucleation density and a corresponding increase in grain size, giving rise to a good bilayer MoS2 film [Fig. 3(h)]. However, if the temperature is too high (960 °C), the oxygen-induced etching begins to dominate. The enhanced etching effect of oxygen would lead to a further decrease in the nucleation density and thus a discontinuous bilayer MoS2 film [Fig. 3(i)].

    The effect of the growth time on the growth of multilayer MoS2 is studied by changing the growth time from 5 min to 35 min while keeping other growth parameters unchanged, as shown in Figs. 3(j)–3(l). When the growth time is 5 min, the coverage of bilayer MoS2 is low and only ∼ 30% [Fig. 3(j)]. With the extension of the growth time to 15 min, the bilayer MoS2 domains are spliced into a continuous film with only a few trilayer grains with the size of ∼ 4 μm [Fig. 3(k)]. Increasing the time further, trilayer MoS2 gains would emerge [Fig. 3(l)].

    Bilayer and trilayer MoS2, compared to monolayer ones, in principle show improved electron mobilities and therefore provide a more promising platform in terms of device applications. To confirm this, we hence fabricate the flexible FETs array on PET flexible substrates [Fig. 4(a)]. Figure 4(b) illustrates the device geometry with Ti–Au–Ti as the local back-gate electrode, 20 nm atomic-layer-deposited-Al2O3 as dielectric layer, gold (Au) as contact and monolayer/bilayer/trilayer MoS2 as the semiconductor channel. Figure 4(c) presents the room temperature output curves of flexible back-gate devices based on bilayer MoS2 with channel L/W of 5 μm/10 μm. under different back-gate voltages Vg. The overall linear output characteristics suggest the low-resistance ohmic contact behavior. The transfer curves of the monolayer, bilayer, and trilayer FETs are illustrated in Fig. 4(d). Clearly, with increasing the layer number, the on-state currents increase monotonically, while the on/off ratio decreases from ∼ 108 to ∼ 106. Furthermore, the field-effect mobility μ is extracted by μ=GmLWCiVds, where Gm is the transconductance, Ci denotes the gate capacitance, Vds is the source–drain bias, L and W are channel length and width, respectively. Figure 4(e) summarizes the electron mobility of flexible monolayer (upper panel), bilayer (middle panel), and trilayer MoS2 devices (lower panel). The average mobility of the bilayer (trilayer) MoS2 is ∼ 16 cm2⋅V−1⋅s−1 (∼ 23 cm2⋅V−1⋅s−1), which shows 45.5% (109.1%) improvements compared with flexible FETs based on monolayer films (i.e., the mobility is ∼ 11 cm2⋅V−1⋅s−1).

4.   Conclusion
  • In summary, we design a two-step OA-CVD methodology and synthesize 4-inch MoS2 films from monolayer to trilayer on sapphire substrates. Compared with the previous one-step synthesis method, our two-step OA-CVD strategy can precisely control the growth of each layer independently, thus facilitating the possibility to investigate the growth parameters on the growth of multilayer MoS2. The influence of the evaporation temperature, the oxygen flow rate, the growth temperature and the growth time on the growth of multilayer MoS2 is systematically explored. Flexible FETs fabricated from bilayer (trilayer) MoS2 show significant improvements in device performances compared with flexible FETs based on monolayer films. Our work provides new insights into the study of growth regulation and controlled synthesis of multilayer 2D van der Waals materials.

Data availability
  • The paper and the supplementary information file provide pertinent data that support the study’s main conclusions. The authors of the corresponding study have made all of the raw data produced during this investigation available upon request.

Figure (4)  Reference (36)