HTML
-
Permanent magnetic materials are indispensable in a wide range of applications, including electric motors, generators, and magnetic storage devices.[1–3] The development of high-performance magnets with enhanced intrinsic and extrinsic properties is a persistent challenge in materials science, particularly for iron-rich rare-earth magnets, which have garnered significant interest due to their potential to offer superior magnetic properties.[4–9] Among these, ThMn12-type rare-earth permanent magnets have emerged as a promising candidate because of their excellent intrinsic magnetic properties, including high magnetization and high anisotropy field.[10–13] These characteristics make ThMn12-type magnets an attractive alternative to traditional NdFeB and SmCo magnets, particularly due to their cost-effectiveness and environment-friendly properties.[9,14,15]
ThMn12-type magnets exhibit great potential for advanced magnetic applications, but their practical implementation faces significant challenges rooted in intrinsic metastability and structural controllability. The metastable nature of the ThMn12-type phase fundamentally disrupts crystallization kinetics during synthesis, while the inherently small single-domain grain size imposes additional constraints on microstructure engineering.[16,17] Generally, these intrinsic characteristics create dual obstacles: they not only impede the attainment of required phase purity but also promote unintentional coexistence of hard and soft magnetic phases — a critical issue when pursuing nanocrystallization strategies to enhance magnetic performance.[18–20]
In conventional permanent magnets, nanocrystallization enhances functional properties through two well-established mechanisms: (i) domain wall pinning at refined grain boundaries for increased high coercivity (Hc),[21–23] and (ii) directional magnetization reversal governed by grain size disparity for higher energy density.[24] However, in ThMn12-type systems, unpredictable phase transitions during processing lead to erratic grain growth dynamics, making it exceptionally difficult to achieve both narrow size distributions and spatially ordered magnetic domains.[17,25] Unlike stable magnetic compounds where thermal treatments can systematically tune nanostructures, the transient crystallization pathways in ThMn12-type materials often result in disordered domain configurations that negate the theoretical benefits of nanocrystallization.
This contradiction arises from competing requirements: the thermodynamic instability demanding rapid solidification to preserve the desired phase, versus the kinetic necessity for controlled crystallization to establish ordered nanostructures.[26–30] Consequently, achieving stable and high-performance magnets has been a significant challenge in previous research efforts.
Several approaches have been explored to address these issues, including compositional modifications and the introduction of doping elements to stabilize the ThMn12-type phase. Most studies tend to increase the stability of the ThMn12-type structure by adding stability-enhancing elements; however, this often results in a significant decrease in magnetization, as observed with the substitution of Fe by Ti, V, Cr, Mn, Mo, W, Si, and Al.[31–42]
Few reports reveal that B can form B-rich boundary phases at the grain boundaries of ThMn12-type films, which serve to magnetically isolate the grains.[43,44] In the context of ribbons, B appears to induce the precipitation of Ti-rich phases or grain refinement, thereby enhancing the magnetic performance of the samples.[45,46] This suggests that B has a significant effect on the modification of grain boundaries, which is closely related to the Hc of ThMn12-type magnets. However, whether B plays additional roles in ThMn12-type magnets remains unclear, presenting considerable research value for further exploration.
Furthermore, relatively little research has focused on the control of ThMn12-type magnets’ microstructure and the simplification of the overall fabrication process. In traditional methodologies, the preparation of nano/microcrystalline magnets typically follows one of two approaches: the first involves melting, homogenization, and refinement;[47] the second involves melting, amorphization, and grain growth.[48] The distinction lies in whether nano/microcrystals are formed directly or whether existing large particles are refined to produce nano/microcrystalline magnets or magnetic powders. However, the complex preparation steps hinder potential industrial-scale production of the metastable ThMn12-type magnets. Therefore, simplifying the fabrication process and addressing the metastable characteristics of ThMn12-type magnets are the critical factors in developing this magnet, which is valuable for both scientific research and industrial application.
In this study, ThMn12-type Sm0.8Zr0.2Fe11SiBx (x = 0–0.2) ribbon magnets were successfully synthesized through a one-step rapid solidification process. The introduction of B into the alloy composition significantly enhanced the phase stability of the ThMn12-type structure, enabling the direct formation of a high-purity phase. Furthermore, by carefully optimizing the B concentration and cooling rate, we achieved a uniform microstructure along with improved magnetic properties, including a Hc of 6222 Oe, a remanence (Mr) of 80 emu/g, and a remanence ratio (Mr/Ms) of 0.71. These findings highlight the effectiveness of B doping and one-step processing in addressing the challenges of phase instability and complex preparation requirements, offering a promising strategy for the scalable production of ThMn12-type magnets with high performance and simplified fabrication processes.
-
Ingots with nominal compositions, Sm0.8Zr0.2Fe11SiBx (x = 0–0.2), were prepared by arc-melting high-purity Sm (99.9%), Zr (99.9%), Fe (99.9%), Si (99.9%), and Fe–B (weight fraction ratio of 8:2, 99%) pieces under an Ar atmosphere (99.999%). An excess of Sm of 30 at.% was included in the alloys to compensate for Sm evaporation loss and obtain a high-purity ThMn12-type phase. The ingots were melted in an Ar environment in quartz nozzles and ejected through a 0.4 mm orifice using pressurized Ar gas (99.999%) onto a copper wheel rotating at 20–35 m/s.
The crystal structure and phase purity of the resulting products were examined by x-ray diffraction (XRD) with Cu Kα radiation (λ = 1.5406 Å). The cross-sectional morphologies of the bulk samples were scrutinized with a field emission scanning electron microscope (FE-SEM). The magnetic characteristics of the samples were measured with a physical property measurement system (PPMS) from Lakeshore.
-
Figure 1 presents the XRD results of three samples with varying B contents after ribbon casting at different wheel speeds. As shown, an increase in wheel speed accelerates the cooling rate from the molten state, and amorphization was more severe, with the sample at 35 m/s effectively transitioning to an amorphous state. This behavior aligns with the typical characteristics of ThMn12-type ribbons during rapid solidification.
When comparing the three samples with different B contents at the same wheel speed, it is evident that increasing B content leads to notable differences in phase formation. Overall, higher B concentrations facilitate the transition of samples to an amorphous state or result in finer grain sizes under identical rapid solidification conditions. This effect can be attributed to B acting as an amorphizing agent, which effectively suppresses grain growth during the rapid solidification process. This characteristic underpins our decision to utilize B to induce the formation of ThMn12-type grains.
From Fig. 1, it is evident that at a wheel speed of 20 m/s, the B0 and B0.1 samples primarily form the TbCu7-type phase, with a small amount of α-Fe phase observed in the B0 sample. When the wheel speed increases to 30 m/s, clear diffraction peaks appear at 42.222°, 42.481°, and 43.249°, which indicates the appearance of ThMn12-type Sm0.8Zr0.2Fe11SiBx. As the wheel speed further increases to 35 m/s, the B0 sample exhibits a mixture of amorphous and ThMn12-type phases, while the B0.1 sample is almost entirely amorphous. For the B0.2 sample, a clear presence of a mixed phase of amorphous and ThMn12-type phases is evident at 20 m/s, and complete amorphization occurs at both 30 m/s and 35 m/s.
These observations suggest that the addition of trace amounts of B effectively inhibits the crystallization of the ThMn12-type phase during rapid solidification. Such suppression is beneficial for achieving nanocrystalline ThMn12-type grains while avoiding the formation of significant amounts of α-Fe soft magnetic phase, thereby ensuring the purity of the ThMn12-type phase within the samples.
Figure 2 presents the magnetic performance testing results of samples with three different B contents, cast at varying wheel speeds. The data indicate that the magnetic properties are optimal at a wheel speed of 30 m/s. This can be attributed to two factors: first, the samples prepared at 20 m/s contain a significant amount of the TbCu7-type phase and a small amount of α-Fe phase; second, the samples cast at 30 m/s likely have a more suitable grain size compared to those produced at 20 m/s. Conversely, at a wheel speed of 35 m/s, many samples exhibit signs of amorphization, leading to a decline in magnetic performance. Therefore, our discussion primarily focuses on the magnetic properties and microstructure of the samples prepared at 30 m/s. Respectively, the Hc values for the B0 and B0.1 samples reached 3912 Oe and 6222 Oe at a wheel speed of 30 m/s. The introduction of trace amounts of B significantly enhances the Hc, yielding an increase of approximately 59%. Due to trace element doping, such a substantial increase in Hc is relatively rare; most studies on ThMn12-type materials have primarily adjusted Hc through significant changes in grain size and alloy composition.
The XRD results confirm that trace B doping has a pronounced effect on inhibiting grain growth, suggesting that B plays a crucial role in optimizing Hc. However, aside from inhibiting grain growth, it remains unclear whether other effects are present that may influence magnetic properties, particularly regarding the sample’s crystal structure and microstructure. Therefore, further investigation is warranted to elucidate the additional impacts of B on the magnetic performance of the samples, as this may reveal further avenues for optimizing magnetic properties.
Figure 3 presents the magnetization versus temperature (MT) curves of the B0, B0.1, and B0.2 samples prepared at a wheel speed of 30 m/s. The XRD patterns from Fig. 1 indicate that the peak intensities of the nanocrystalline/amorphous samples are insufficient to accurately determine whether B directly affects the crystal structure of the ThMn12-type phase. Therefore, MT measurements were conducted to assess whether the Curie temperature (Tc) varies significantly with the addition of B.
The results indicate that the Tc of the B0 and B0.1 samples are relatively similar, suggesting that their crystal structures do not exhibit significant changes. However, the MT curve for the B0 sample shows some optimization, which may be attributed to its lower purity compared to the B0.1 sample, resulting in the presence of minor secondary phases. The reduction of these secondary phases could be one of the factors contributing to the optimization of the magnetic properties.
In contrast, the Tc of the B0.2 sample is significantly lower than that of the B0 and B0.1 samples. This can be attributed to the fact that the B0.2 sample is nearly entirely amorphous, and the Tc of amorphous samples typically differs considerably from that of ThMn12-type materials. This observation reinforces the notion that the structural characteristics of the samples play a crucial role in determining their magnetic behavior. Further investigation into the relationship between the amorphous nature and magnetic properties of the B0.2 sample is warranted to fully understand these dynamics.
Figure 4 presents FE-SEM images for the B0, B0.1, and B0.2 samples prepared at a wheel speed of 30 m/s. As confirmed in Fig. 3, trace amounts of B do not appear to have a significant effect on the ThMn12-type crystal structure, suggesting that the changes in Hc are not attributable to alterations in crystal structure. Consequently, FE-SEM analysis was conducted to investigate whether the microstructural characteristics of the samples had undergone changes.
The images were taken from the vertical cross-sections of the ribbon samples, which were freshly exposed by breaking the ribbons rather than by polishing. Polishing was avoided due to the excessively fine grain sizes, which would obscure useful information. At low magnifications, the FE-SEM images reveal significant differences in the cross-sectional structures of the three samples, with the only variable being the trace B doping. The B0 sample exhibits a generally uniform and smooth morphology; however, certain regions display pronounced differences in brightness, indicating compositional variations. This segregation is attributed to the metastable characteristics of the ThMn12-type structure during the rapid solidification process, which affects the final consistency of the samples and consequently influences their magnetic properties.
In contrast, the B0.1 sample shows substantial changes in microstructure. Upon magnification of specific regions, a uniformly fine-grained structure becomes apparent. These structures are likely formed during fracture, indicating multiple fine interface layers. During the fracture process, the differing stress distributions within these layers and the grain interiors produce a serrated morphology. The abundance of interfaces may contribute to the significant increase in Hc observed in the B0.1 sample, as these interfaces can act as pinning sites during magnetization reversal, impeding the process and thereby enhancing Hc.
When the B content is increased to 0.2, the distinctive fine-grained structure disappears, leaving only smaller grain features that are barely discernible. Comparison with the XRD results indicates that the B0.2 sample has nearly transformed into an amorphous state during rapid solidification, making it challenging to identify any distinct fine-grained or interface morphology in the cross-section. This observation underscores the impact of B doping on the microstructural evolution and magnetic properties of ThMn12-type magnets.
-
This work primarily investigates the changes in magnetic properties of ThMn12-type ribbon samples with the alloy composition Sm0.8Zr0.2Fe11SiBx (x = 0–0.2) under varying cooling rates (wheel speeds of 20–35 m/s) and different B contents. The sample Sm0.8Zr0.2Fe11SiBx, subjected to rapid solidification at a wheel speed of 30 m/s, successfully achieves Hc, Mr, and Mr/Ms values of 6222 Oe, 80 emu/g, and 0.71, respectively. This study identifies and explores the effects of B on inhibiting grain growth of the ThMn12-type phase, its role in suppressing segregation during rapid solidification, and its impact on optimizing microstructure. The findings suggest that trace amounts of B can significantly enhance the magnetic performance of ThMn12-type magnets produced via rapid solidification, and indicate potential unknown effects that warrant further investigation.
首页