2025 Volume 34 Issue 11
Article Contents

Jiufang Han, Yimeng Song, Xiran Yu, Conghui Jiang, Wenxin Wang, Haiqiang Jia, Chunhua Du, Hong Chen. Thorough numerical simulations of silicon heterojunction solar cells focusing on the sun-side-doped layer[J]. Chinese Physics B, 2025, 34(11): 118801. doi: 10.1088/1674-1056/addcc4
Citation: Jiufang Han, Yimeng Song, Xiran Yu, Conghui Jiang, Wenxin Wang, Haiqiang Jia, Chunhua Du, Hong Chen. Thorough numerical simulations of silicon heterojunction solar cells focusing on the sun-side-doped layer[J]. Chinese Physics B, 2025, 34(11): 118801. doi: 10.1088/1674-1056/addcc4

Thorough numerical simulations of silicon heterojunction solar cells focusing on the sun-side-doped layer

  • Received Date: 22/04/2025
    Accepted Date: 22/04/2025
    Available Online: 01/11/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(5)  /  Tables(2)

Article Metrics

Article views(319) PDF downloads(1) Cited by(0)

Access History

Thorough numerical simulations of silicon heterojunction solar cells focusing on the sun-side-doped layer

Abstract: To improve the photovoltaic conversion efficiency (PCE) of silicon heterojunction (SHJ) solar cells, this study focuses on optimizing the physical parameters of the sun-side-doped layer and proposes strategies to address the challenges posed by Fermi level pinning in wide bandgap designs. Using AFORS-HET simulations, we systematically investigate the effects of bandgap width, doping concentration, and defect state distribution on the energy band structure, interface electric field, and carrier transport dynamics. The results reveal that maintaining the Fermi level within 0.3 eV of the conduction band is essential for optimal device performance. A wider bandgap (> 1.8 eV) enhances the utilization of short-wavelength light and significantly suppresses interface recombination, leading to an increase in short-circuit current density (Jsc) by 0.8 mA/cm2. This benefit comes with a delicate balance between minimizing defect state density and improving doping efficiency. This study provides theoretical insights into the optimization of doped layer physical parameters and proposes practical solutions, including nano-crystallization and low-doping interface strategies, to improve the performance of SHJ solar cells and support industrial applications.

1.   Introduction
  • Silicon heterojunction (SHJ) solar cells have emerged as leading candidates for high-efficiency photovoltaic devices due to their superior photoelectric conversion efficiency (PCE) and potential for cost-effective manufacturing.[1–3] As commercialization advances, SHJ solar cells consistently set new PCE records.[4] However, the actual efficiency still falls short of the theoretical limit of 28.5% for SHJ solar cells.[5–7]

    Addressing this challenge requires continuous advancements in materials and device designs, particularly in optimizing the doped layers on the sun side, which play a critical role in light absorption, carrier transport, and interface recombination control.[3,8,9] An optimal-doped layer should: (i) have a low optical absorption coefficient to minimize parasitic absorption; (ii) exhibit low activation energy and defect density to reduce recombination and enhance carrier transport; (iii) feature a band offset that facilitates selective carrier extraction. Extensive studies have explored the use of alternative materials to hydrogenated amorphous silicon (a-Si:H), including hydrogenated amorphous silicon carbide (a-SiCx:H) and hydrogenated amorphous silicon oxide (a-SiOx:H), to mitigate parasitic absorption and enhance carrier collection.[10–12] Incorporating nanocrystals further reduces the absorption coefficient while enhancing doping efficiency and conductivity.[12,13] Replacing a-Si:H with a-SiOx:H films reduces short-wavelength absorption coefficients, increasing short-circuit current density (Jsc) by 0.13 mA/cm2.[14] A dual-layer doped structure based on p-nc-SiOx:H and p-nc-Si:H facilitates efficient hole collection, achieving an SHJ solar cells with a fill factor (FF) ranging from 83%–86%.[15] Using p-nc-Si:H thin layers grown by VHF-PECVD as the sun-side-doped layer increases Jsc due to reduced parasitic absorption, while improving open-circuit voltage (Voc) and FF due to better passivation and electrical contact, leading to a PCE improvement of 7.2%.[16] Additionally, employing n-nc-SiOx:H as the front-doped layer minimizes parasitic absorption, resulting in a PCE of 26.74% and a Jsc of 41.16 mA/cm2.[17]

    Optimizing doped layer materials requires a balanced consideration of multiple physical properties. For instance, reducing optical absorption to suppress parasitic losses often demands widening the bandgap, while enhancing conductivity may involve introducing nanocrystallinity. These strategies, however, can simultaneously alter the electronic band structure of the doped layer, including not only the bandgap width but also the absolute positions of the valence and conduction bands. Such changes inevitably affect the band alignment at the SHJ device interface and influence carrier transport dynamics.[18,19] Therefore, precise control over the physical parameters of the doped layer is essential to ensure optimal device performance, and the need for a systematic investigation into the physical properties of doped layers is highlighted.

    This work focuses on addressing the limitations imposed by Fermi-level pinning in wide-bandgap-doped layers, which restrict their practical application despite their theoretical advantages. To overcome the high costs associated with experimental iterations, we employ AFORS-HET software to simulate SHJ solar cells.[20–22] This software facilitates precise parameter optimization and comprehensive evaluation of strategies for enhancing PCE.[23–25] We systematically investigate the effects of bandgap width, doping concentrations, and defect state distributions on the energy band structure, carrier transport, and recombination dynamics. Our results highlight the potential of wide-bandgap-doped layers to reduce parasitic absorption and enhance carrier extraction efficiency. Furthermore, we propose physical optimization strategies, including defect state management and doping control, to mitigate Fermi-level pinning. We also introduce design principles involving nano-crystallization and buffer-layer approaches to minimize recombination losses and improve PCE. These findings offer a new perspective on doped-layer engineering and provide practical guidelines for optimizing SHJ solar cell performance.

2.   Methods
  • A set of a-Si:H and a-SiCx:H films were prepared using silane (SiH4), methane (CH4), and hydrogen (H2) gases in a capacitively-coupled PECVD (13.56 MHz) system, maintaining a working pressure of 120 Pa. The films were grown on glass substrates, using applied RF power of 25 mW⋅cm−2, at a low growth temperature of ∼ 200 °C. The samples were grown with the varying H2-dilution ratio R(H2) = [H2]/[SiH4+CH4] from 5 to 120 and CH4 ratio R(CH4) = [CH4]/[SiH4] from 0 to 2. The initial base vacuum in the PECVD reactor before plasma ignition was retained at ∼ 10−5 Pa. The typical thickness of the samples deposited on the glass substrates was maintained at 40 nm–200 nm. If a post-annealing process is mentioned, the annealing is carried out in a nitrogen atmosphere at a temperature of 300 °C for 2 hours. The optical transmission data were recorded using a Shimadzu UV-3600i Plus, UV-VIS-NIR spectrophotometer. The crystallinity of the grown film network was estimated using a Raman spectrometer (Jobin Yvon JY-T64000) with a 532-nm laser at a low power density of ∼ 2 mW⋅cm−2.

    When performing simulations of SHJ solar cells, the distribution of carriers and electric fields inside the solar cell is obtained by solving a set of partial differential equations, including the one-dimensional (1D) Poisson’s equation and the continuity equations.

    The 1D Poisson’s equation, which is to be solved at each x, reads

    where εr and ε0 are the relative and vacuum dielectric constants, q is the electron charge, p and n are the hole and electron densities, ND and NA are the donor and acceptor doping concentrations, and ρtrap is the total charge trapped by defects. And the 1D continuity equations are

    where G is the carrier generation rate, R is the carrier recombination rate, and j is the current density.

    To investigate the impact of physics parameters of the sun-side-doped layer on SHJ solar cell performance, an n-SiCx:H layer will be introduced into the simulated structure as the doped layer on the sun side, as the basis of all the parameter changes. Additionally, the insertion of a hydrogenated intrinsic amorphous silicon (i-a-Si:H) layer between the p-c-Si wafer and doped layer (n-SiCx:H or p-a-Si:H) was considered. The focus of our investigation was on the band gap width, defect state distribution, and doping level of the n-SiCx:H layer. Figure 1(a) is a schematic diagram of the simulated SHJ solar cell structure. The SHJ solar cells were simulated based on p-doped monocrystalline Si wafers (150 μm).

    In the simulation, AM 1.5 radiation was used as the illumination source with a power density of 100 mW⋅cm−2. The main simulated parameters of the different layers are listed in Table 1.[26,27] The main defects of a-Si:H and n-SiCx:H deposited by PECVD include band tail states caused by periodic damage and dangling bonds incompletely passivated by hydrogen atoms, which were characterized by the Urbach tail and Gaussian models, as shown in Fig. 1(b). It was assumed that the position of the characteristic energy of the Gaussian defect state in the band gap is linearly related to the width of the band gap. The position of characteristic energy (calculated from the characteristic energy to the conduction band bottom), along with the specific values of the total density of different defect states are provided in Table 2. Meanwhile, the band tail states are set to fixed values.

    For the p-c-Si substrate, oxygen defects with a density of 1 × 1010 cm−3⋅eV−1, located at 0.56 eV above the valance band top, were assumed. A flat band was applied to the front and back contacts to negate any contact potential. The surface recombination velocity of both electrons and holes was set at 1 × 107 cm⋅s−1. During the simulation process, all these parameters were taken into account except for instances where specific variables were to be considered.

3.   Results
  • We used the UV-VIS-NIR transmittance data of the prepared a-SiCx:H, a-Si:H, and μc-Si:H thin films to investigate their optical properties across a range of gas flow ratios, which are detailed in Fig. 1(c). Tauc’s relation was employed to estimate the optical bandgap of the films, and the Urbach energy can also be obtained by fitting the optical absorption spectrum.[28] Figure 1(c) shows that as the R(CH4) increases from 0 to 2, the optical bandgap of the films rises from 1.78 eV to 2.05 eV. When R(H2) reaches 120, the optical bandgap dramatically increases to 2.25 eV, without the presence of CH4 gas. In films that underwent low-temperature annealing after deposition, the optical bandgap decreases to 1.50 eV, with the lower inverse slope reflecting an increase in disorder due to the removal of H atoms.[29] The corresponding Urbach energy increases with increasing R(CH4), decreases with increasing R(H2), and also decreases after annealing, ranging from 63 meV to 342 meV.

    Figure 1(d) presents the Raman spectra of the Si–Si bonding band in μc-Si:H films prepared at different H2 dilution ratios, R(H2) = 50 and 120. The main peak are at ∼ 480 cm−1 for the a-Si–Si component, ∼ 501 cm−1 for the nc-Si–Si component, and at ∼ 520 cm−1 for the c-Si–Si component.[28] As R(H2) increases, the relative area ratio of the a-Si–Si component peak decreases, while the crystalline component grows. The crystallization rate is calculated based on the ratio of the crystalline component peak area to the total peak area. Across the range of R(H2) from 5 to 120, the crystallization rate varies from 0 to 76.20%. The physical parameters measured from all the films provide a basis for numerical simulations described later.

    We conducted numerical simulations to investigate how variations in bandgap width, doping concentration, and defect state distribution influence the Fermi-level position and overall device performance. Figure 2 illustrates the simulation results based on two defect density groups, D1 and D3, with doping concentrations ranging from 1 × 1019 cm−3 to 1 × 1021 cm−3.

    For low-defect density layers (D1 group), devices with doping concentrations below 5 × 1019 cm−3 exhibited a sharp drop in both Voc and FF as the bandgap widened from 1.4 eV to 2.2 eV. This parameter region is referred to as a dead zone in this article, as indicated by the dashed box in Fig. 2. While, higher doping levels (> 5 × 1019 cm−3) successfully suppressed the dead zone, enabling stable performance even at wider bandgaps.

    Compared with the D1 group, the simulation results of the high-defect density group (D3) exhibit a similar variation trend, as shown in Fig. 2(b). However, the doping level required for SHJ solar cells to avoid the dead zone significantly is significantly higher in the D3 group. With increasing bandgap width, this required doping level continues to rise. Specifically, unlike the D1 group, where lower doping concentrations maintain stable performance, the D3 group requires a doping concentration of 1 × 1020 cm−3 to sustain normal efficiency at bandgaps of 1.4 eV and 1.6 eV. Beyond this range, as the bandgap increases, the overall efficiency sharply decline, leading to the formation of a dead zone. The formation of the dead zone and its deep relationship with the position of the Fermi level will be further discussed later.

    Furthermore, when the doping concentration exceeds a certain threshold, above 5 × 1019 cm−3 for the D1 group and above 5 × 1020 cm−3 for the D3 group, the efficiency curves of the solar cells split into two distinct groups, with efficiencies of 25.0% and 25.5%, respectively. This divergence is more pronounced in the magnified images embedded in Figs. 2(a) and 2(b), which is mainly attributed to the difference in Jsc. Similar trends can be observed in the magnified Jsc curves for the D1 and D3 groups. To further investigate these phenomena and provide practical guidance for optimizing solar cell design and fabrication, a more detailed analysis is presented in the subsequent sections.

4.   Discussion
  • To investigate the origin of the dead zone, we performed detailed simulations focused on the boundary region of the D3 group, specifically SHJ solar cells with a doping concentration of 1 × 1020 cm−3. Figure 3(a) displays the I–V and P–V curves under illumination, with P–V curves shown in lighter shades for clarity. As the bandgap widens, the Jsc in the I–V curves exhibits a slight increase. However, a gradual transition from a standard I–V shape to an S-shaped curve is observed. This S-shaped distortion shifts the power peak leftward in the P–V curves, reducing the FF from 82.1% at 1.4 eV to 65.6% at 2.2 eV. Previous studies attribute this phenomenon to band mismatches at the heterojunction interface.[30]

    Figure 3(b) further illustrates the distribution of n-type carriers within the doped layer as a function of bandgap width. A larger bandgap reduces the carrier concentration, impairing transport efficiency and lowering overall device performance.

    Variations in bandgap width, doping levels, and defect distributions directly influence the Fermi level position, as shown in the heatmap in Fig. 3(c). The energy difference (δE) between the Fermi level and the conduction band edge decreases as the color transitions from red to blue. In Fig. 3(c), the dashed region highlights the parameter range associated with the dead zone observed in Fig. 2(b). Devices enter the dead zone when δE exceeds 0.3 eV, whereas maintaining δE below this threshold (blue regions) prevents performance degradation. This highlights the strong correlation between Fermi-level position and the performance of the SHJ device.

    As the bandgap widens, the likelihood of Fermi-level pinning increases due to the displacement of dangling bond energy levels further from the conduction band. This necessitates higher doping concentrations to compensate for defect states, creating a delicate tradeoff between minimizing defect density and enhancing doping efficiency.

    Figure 3(d) presents the corresponding band diagrams for varying bandgap widths. The conduction band offset (marked by double arrows) decreases as the bandgap widens, contributing to the development of the S-shaped I–V curves and further reductions in FF.[31]

    While widening the bandgap reduces parasitic absorption and optical losses, it introduces structural challenges that require careful consideration. Specifically, higher doping concentrations may increase defect densities, leading to stronger Fermi-level pinning and performance degradation.

    Although the simulated doping concentrations range from 1 × 1019 cm−3 to 1 × 1021 cm−3, we emphasize that this analysis serves as a qualitative investigation to capture general trends in electrical behavior. In deposition processes, the total number of dopant atoms introduced into the film can indeed reach the 1021 cm−3 level. However, in amorphous and nanocrystalline silicon, the effective doping efficiency is typically limited due to compensation by defect states, resulting in the Fermi level remaining not less than 0.1 eV away from the conduction or valence band edges. Nevertheless, recent studies have demonstrated that post-deposition treatments such as light soaking can significantly enhance dopant activation and improve effective doping in hydrogenated amorphous silicon, suggesting potential pathways to overcome this limitation in practical applications.[32] In practical scenarios, figure 4(a) shows that defect state densities scale linearly with doping concentrations, ranging from D1 to D5. As depicted in Fig. 4(b), this correlation amplifies Fermi-level pinning effects, particularly in wide-bandgap configurations. Therefore, optimizing doping profiles and minimizing defect densities through nano-crystallization techniques is essential for maintaining electrical performance.

    To further investigate the underlying mechanisms responsible for the bifurcation of solar cell efficiency curves into high- and low-performance categories as the bandgap width varies, we performed detailed simulations. We simulated the external quantum efficiency (EQE) curves, shown in Fig. 5(a), which revealed a distinct segmentation in EQE behavior as the bandgap width varied. Notably, SHJ solar cells with larger bandgaps exhibited higher EQE values, especially in the short-wavelength region.

    We also simulated the evolving trends of Jsc and PCE under different bandgap widths while maintaining the defect state distribution of D1 and a doping concentration of 1 × 1020 cm−3, as shown in Fig. 5(b). A sharp performance transition was observed around a bandgap width of 1.7 eV.

    The differences in EQE at short wavelengths primarily result from variations in parasitic absorption and carrier transport dynamics in the light-receiving regions. Figure 5(c) illustrates the corresponding band diagrams of the sun side under different bandgap conditions. As the bandgap of the doped layer increases, the relative alignment between the valence band of the doped layer and the intrinsic layer shifts. Specifically, at 1.4 eV and 1.6 eV, the valence band of the doped layer lies above that of the intrinsic passivation layer. However, when the bandgap widens to 1.8 eV, the positions are reversed. Simultaneously, the quasi-Fermi level gradient for holes at the interface is inverted, which facilitates the extraction of photogenerated carriers from the illuminated surface region (including the doped and passivation layers). This trend is consistent with the EQE results shown in Fig. 5(a). Notably, a sharp improvement in Jsc is observed when the bandgap reaches around 1.7 eV, which corresponds to a critical transition point in the interface band alignment. This transition enhances carrier selectivity and extraction efficiency, especially in the front-side layers, contributing to the observed performance jump.

    Figures 5(d) and 5(e) illustrate the simulated carrier distributions and recombination rates for bandgap widths of 1.6 eV and 2.0 eV, respectively. In structures with narrower bandgaps, insufficient band offsets lead to potential barriers that trap minority carriers at the interface, causing elevated recombination rates. In contrast, wider bandgaps reduce carrier recombination, resulting in more efficient carrier extraction.

    These simulations highlight that wider bandgap-doped layers significantly enhance carrier extraction and separation on the sun side, particularly for short-wavelength light. The improved transport dynamics and reduced recombination losses, observed through EQE and recombination rate analyses, underscore the potential of wide-bandgap materials to optimize SHJ solar cell performance. However, it should be noted that the AFORS-HET simulation tool used in this study does not explicitly account for tunneling effects, particularly those assisted by band tail states. This limitation may lead to discrepancies between simulation and real device performance, especially under strong interfacial electric fields or large band offsets where tunneling plays a non-negligible role.

    As discussed earlier, incorporating a wider bandgap in the sun-side-doped layer significantly enhances carrier transport and separation at the front surface, thereby improving the overall photoelectric conversion efficiency of SHJ photovoltaic devices. However, the use of wide-bandgap materials also increases the likelihood of Fermi-level pinning, particularly when compared to traditional a-Si:H doped layers. This effect can degrade device performance, emphasizing the need for careful material and process optimization.

    Simulations reveal that achieving optimal performance with wide-bandgap doped layers requires a delicate balance between minimizing defect state density and optimizing doping efficiency. Specifically, Fermi-level pinning becomes more pronounced as the bandgap widens, necessitating higher doping concentrations to compensate for defect states and avoid performance degradation. At the same time, excessive defect densities amplify recombination losses, especially at the interface between the wide-bandgap doped layer and the a-Si:H passivation layer. Despite these challenges, wider bandgaps effectively reduce parasitic absorption and improve short-wavelength utilization, provided that a stable band alignment and low recombination rates can be maintained.

    To address these challenges, several optimization strategies can be employed. Nano-crystallization has proven to be an effective approach, as it reduces the density of dangling bonds, enhances doping efficiency, and improves doping levels at the same concentration. Additionally, interface engineering is critical for mitigating recombination losses caused by band offsets at the interface between the doped layer and the passivation layer. As shown in Fig. 5, reducing the doping concentration at this interface, or introducing a thin intrinsic wide-bandgap buffer layer, can smooth transitions and suppress recombination. Furthermore, strict quality control is essential for wide-bandgap doped layers, as their photosensitivity serves as a key metric for evaluating material performance. These insights highlight the importance of carefully engineered materials and deposition processes to balance bandgap widening and carrier transport efficiency.

    The findings above provide clear design principles and process guidelines for optimizing wide-bandgap doped layers in SHJ solar cells. These strategies, derived from systematic simulations, are relatively straightforward to implement in large-scale industrial production. By reducing costs and improving efficiency, these methods are expected to accelerate the commercialization of SHJ photovoltaic technologies.

5.   Conclusion and perspectives
  • The results demonstrate that wider bandgap doped layers in SHJ solar cells effectively optimize carrier extraction on the sun side while reducing parasitic absorption. Simulation data indicate that these layers are more susceptible to Fermi level pinning caused by excessive defect states. When the Fermi level is maintained within 0.3 eV of the conduction band, the adverse effects of Fermi level pinning on device performance is significantly reduced. Consequently, the critical role of nano-crystallization in enhancing the applicability of wide-bandgap-doped layers is highlighted. Additionally, the introduction of lower doping levels or intrinsic transition layers within wide-bandgap-doped layers is proposed as a viable strategy to optimize carrier extraction and concurrently suppress carrier recombination.

Figure (5)  Table (2) Reference (32)