2025 Volume 34 Issue 10
Article Contents

Jinghua Ren, Yuelin Zhang, Miming Cai, Yuhan Li, Mingming Li, Tianqi Wang, Dekun Shen, Hongyu Zhou, Xiangwei Zhu, Jinxing Zhang. Temperature and angle dependence of magnetic damping in manganite thin films[J]. Chinese Physics B, 2025, 34(10): 107504. doi: 10.1088/1674-1056/ade06d
Citation: Jinghua Ren, Yuelin Zhang, Miming Cai, Yuhan Li, Mingming Li, Tianqi Wang, Dekun Shen, Hongyu Zhou, Xiangwei Zhu, Jinxing Zhang. Temperature and angle dependence of magnetic damping in manganite thin films[J]. Chinese Physics B, 2025, 34(10): 107504. doi: 10.1088/1674-1056/ade06d

Temperature and angle dependence of magnetic damping in manganite thin films

  • Received Date: 31/03/2025
    Accepted Date: 13/05/2025
    Available Online: 01/10/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(4)

Article Metrics

Article views(306) PDF downloads(1) Cited by(0)

Access History

Temperature and angle dependence of magnetic damping in manganite thin films

Abstract: Magnonics and magnonic materials have attracted widespread interest in the spintronics community and demonstrate potential for applications in the next generation of information technology. Recent advances in manganite thin films highlight their promise for magnonics, in which enhanced film quality and strain control of spin and electronic structures play a crucial role in reducing magnetic damping. Here, we report the fabrication of La0.67Sr0.33MnO3 thin films of varying quality via pulsed laser deposition. The quality of epitaxial films is characterized using atomic force microscopy and x-ray diffraction. A pronounced fourfold anisotropy in the magnetic damping (with a ratio of about 150%) is observed, where the minimum damping occurs along the [110] crystalline orientation. Notably, improved sample quality significantly reduces the magnetic damping at low temperatures. The highest-quality sample, featuring atomic-scale terraces, exhibits a magnetic damping of ∼ 2.5 × 10−3 at 5 K. Our results not only demonstrate effective reduction of low-temperature magnetic damping in high-quality correlated oxide systems but also provides a strategy and material platform for exploring novel quantum phenomena and for designing low-temperature magnonic devices.

1.   Introduction
  • Spin waves can propagate over long distances within low-damping magnetic materials without involving electron motion, resulting in minimal heat dissipation. This advantage positions spin waves as promising candidates for next-generation information technology.[1] Consequently, research on magnonic material systems has advanced significantly.[2–4] The perovskite manganite, as a strongly correlated electron system, has attracted extensive attention in spintronics[5] and magnonics[6] due to its unique physical properties and tunability, such as remarkable colossal magnetoresistance,[7] metal–insulator transition[8,9] and nontrivial spin textures.[10,11] Among these, La0.67Sr0.33MnO3 (LSMO) with the doping ratio of 0.33 for Sr exhibits not only an above-room-temperature Curie temperature (∼ 370 K) with excellent ferromagnetic properties but also a half-metallic nature with low residual resistivity (≤ 10−4 Ω⋅cm). The near-complete spin polarization (∼ 100%) of LSMO was reported in spin-polarized photoemission[12] and tunnel magnetoresistance[13] experiments, which establishes a fundamental basis for its applications in spintronic devices.

    Recently, numerous breakthroughs in magnonics have been reported in strained LSMO thin films, including magnetization modulation induced by twinned structural order and magnonic crystals in LSMO/SrTiO3 films,[14] low-density current control of spin wave propagation in LSMO/LaAlO3 films,[15] anisotropic spin-wave propagation,[16] coexisting nonreciprocities of spin-wave propagation originated from strain-driven Dzyaloshinskii–Moriya interaction and the stabilization of topological magnetic skyrmions at room temperature,[11] nonlinear three-magnon scattering between magnon energy bands,[17] and long-distance propagation of chiral magnonic edge states in quasi-antiferromagnetic spin textures.[18] These results provide critical experimental foundations for constructing low-power magnonic integrated circuits.

    The functionality of LSMO has been further enhanced by constructing heterostructures with interface engineering or strain modulation. In multiferroic heterostructures containing ferromagnetic LSMO and ferroelectric BiFeO3 or BaTiO3, magnon–phonon coupling and the long-range propagation of coherent magnon-polaritons have been experimentally observed.[19–21] Spin pumping and interfacial spin transport have been studied in heterostructures containing materials with strong spin–orbit coupling, such as Pt[22,23] and SrRuO3.[24] Interestingly, the extremely long-range Josephson coupling has been demonstrated in LSMO/YBa2Cu3O7 ferromagnet–superconductor heterostructures.[25] These achievements highlight the immense potential of LSMO heterostructures in spintronic and magnonic devices based on magnetoelectric effects and superconductivity.[26] The discovery of the above phenomena has imposed very high requirements on the quality of LSMO films, specifically, the relationship between sample quality and low-temperature damping remains to be systematically studied.

    Here, we report the epitaxial growth of LSMO films with a thickness of ∼ 120 nm on (110)-oriented NdGaO3 (NGO) single-crystal substrates. A remarkable fourfold symmetric anisotropy in the magnetic damping constant is observed in these LSMO/NGO (110) films. Notably, while the room-temperature magnetic damping of all samples falls within a similar range, the highest-quality sample exhibits a significantly lower damping constant of 2.5 × 10−3 at 5 K, which is attributed to the suppression of intraband scattering by improving sample quality.

2.   Experimental methods
  • Single-crystalline epitaxial thin films with high quality are crucial for probing the fundamental properties and mechanisms of phenomena, thereby providing a robust material platform for novel spintronic and magnonic devices. Therefore, we prepared epitaxial LSMO/NGO films, as schematically illustrated in Fig. 1(a). LSMO thin films with a thickness of ∼ 120 nm were grown on NGO (110) substrates by pulsed laser deposition using an excimer laser (248 nm). The substrates were heated to 820 °C, and the films were deposited under an oxygen atmosphere of 23 Pa using a pulsed laser with an energy density of ∼ 0.65 J/cm2 at 5 Hz for 30 minutes. After deposition, the samples were cooled at a rate of 5 °C/min under an oxygen atmosphere of 104 Pa. The crystal structure of sample A was analyzed by x-ray θ–2θ diffraction (XRD) using Cu kα radiation (λ = 0.15406 nm), as shown in Fig. 1(b), which confirms the high-quality single-crystal epitaxy. Bulk LSMO crystallizes in a trigonal structure with a tilted pseudo-cubic unit cell, abulk = bbulk = cbulk = 3.894 Å.[27] The NGO (110) substrate has an orthorhombic crystal structure with a monoclinic pseudo-cubic lattice, abulk = bbulk = cbulk = 3.864 Å. Therefore, the substrate provides in-plane compressive and out-of-plane tensile strains to the LSMO film. The XRD pattern shows the 2θ = 46.42° peak associated with the (002) plane of the LSMO pseudo-cubic phase. The out-of-plane lattice constant c = 3.92 Å was calculated using Bragg’s law.

    The basic magnetic properties of LSMO films were characterized by a vibrating sample magnetometer (VSM). The Curie temperature of sample A was determined to be 371 K by temperature-dependent magnetic moment measurement, as shown in Fig. 1(c). It should be noted that the magnetization of LSMO on the NGO substrate is slightly larger than that on other substrates due to the contribution of the paramagnetic NGO substrate.[28] The in-plane easy axis shows a saturated field of ∼ 40 mT and a coercive field of ∼ 3 mT along the [010]pc orientation, with a saturation magnetization of ∼ 440 emu/cc, as shown in Fig. 1(d). The out-of-plane magnetic hysteresis loop shows a saturated field of ∼ 420 mT and a coercive field of ∼ 2.9 mT along the [001]pc orientation. Previous studies have demonstrated that the distinct lattice constant difference between the a- and b-axes in the NGO substrate induces a uniaxial in-plane compressive strain in the epitaxial LSMO film, which generates a strongly negative perpendicular magnetic anisotropy and a slight in-plane magnetic anisotropy.[11,27]

    The magnetic damping of LSMO thin films was experimentally determined through ferromagnetic resonance (FMR) spectroscopy. The experiments were performed in a commercial physical property measurement system (PPMS) equipped with a superconducting magnet, providing precise control of the applied magnetic field in the in-plane geometry. A high-frequency microwave source was utilized to excite magnetization dynamics through a custom-built broadband coplanar waveguide, while the detection of the resonance signals was achieved using a lock-in amplifier with a diode detector. The in-plane external magnetic field was applied perpendicular to the excitation field from the waveguide.

3.   Experimental results
  • The dynamic magnetic responses of LSMO thin films at room temperature are presented in Fig. 2. The power derivative absorption spectra for a series of fixed excited frequencies f (from 3 GHz to 19 GHz) are displayed in Fig. 2(a), with the sweeping external in-plane magnetic fields applied along the [010]pc orientation. Figures 2(b) and 2(c) show the corresponding frequency dependence of the resonance field and the peak-to-peak linewidth (ΔHpp), respectively. The relationship between the resonance field Hext and the resonance frequency f follows the Kittel mode[29]

    where γ/(2π) = 28 GHz/T is the gyromagnetic ratio, which is estimated from the FMR experimental results. Ms is the saturated magnetization, Hr is the resonance field, and Hani is the anisotropy field. The magnetic damping parameter of LSMO thin films is determined by fitting the frequency dependence of the peak-to-peak linewidths ΔHpp, as shown in Fig. 2(c), extracted from Lorentzian fitting of the derivative absorption spectra, using the following equation:[28,30]

    where ΔH0 is the frequency-independent contribution arising from magnetic inhomogeneities in the LSMO thin films, and α is the intrinsic damping parameter. The damping of α ∼ 1 × 10−3 is estimated by linear fitting of the experimental data as shown in Fig. 2(c), which is slightly larger than values reported in the previous literature with different sample quality.[18] This value is comparable to reports on certain ferromagnetic metals and alloys.[31–33]

4.   Anisotropic magnetic damping
  • The angle-dependent ferromagnetic resonance spectra of sample A are shown in Fig. 3. The measurements were performed at a fixed frequency of 11 GHz, with the external magnetic field rotated between the [010]pc and [100]pc orientations of the LSMO thin film. As illustrated in Fig. 3(a), the resonance peak shifts toward higher magnetic fields as the angle increases from [010]pc to [100]pc, consistent with the expected in-plane magnetic anisotropy.[16] The ferromagnetic resonance spectra at different angles are fitted using Eq. (2). The anisotropy fields along the [010], [110], and [100] orientations are 3 mT, 14 mT, and 30 mT, respectively, as shown in Fig. 3(b). The angular dependence of the resonance field in Fig. 3(c) exhibits two-fold symmetric anisotropy, further confirming the magnetic anisotropy of the LSMO thin film.

    It is also observed in Fig. 3(a) that the resonance linewidth of LSMO thin films exhibits significant angular dependence on the applied in-plane magnetic field. The linewidth reaches a maximum of approximately 8 mT at 0° ([010]pc) and 90° ([100]pc), an intermediate value of ∼ 6 mT at 15° and 60°, and a minimum of ∼ 4 mT at 45° ([110]pc). Furthermore, the anisotropy of the magnetic damping is demonstrated in Fig. 3(d), exhibiting a fourfold symmetry with the minimum damping value observed along the [110]pc orientation. This orientation corresponds to neither an in-plane easy axis nor a hard axis, which is consistent with reported anisotropic spin-wave propagation. The damping constant shows a maximum-to-minimum ratio of ∼ 150% for the 120 nm-thick film. This value is lower than the reported ratio of 200% for spin-wave lifetimes in 20 nm-thick LSMO/NGO films,[16] which is attributed to strain relaxation effects in thicker films.[11] The anisotropy of magnetic damping is influenced by multiple factors, including crystalline symmetry, orientation-dependent spin–orbit coupling (SOC), orbital degrees of freedom, and scattering effects induced by interfacial or bulk defects.[34–37] For instance, the giant damping anisotropy (400%–1400%) observed in CoFe and CoFeAl arises from variations in SOC strength across distinct magnetization orientations, corroborated by anisotropic magnetoresistance (AMR) measurements that highlight the strong correlation between SOC and damping.[34,35] In contrast, CoFeB films exhibit weak AMR–damping correlation (∼ 80%), indicating additional contributions from local lattice distortions or impurity effects.[36] Notably, in Cr/Fe bilayers, a fourfold symmetric damping anisotropy of 400% persists despite negligible magnetocrystalline anisotropy, with no clear AMR–damping relationship.[37] This phenomenon cannot be fully explained by conventional SOC mechanisms or spin-pumping effects. Instead, it has been proposed that orbital Hall effects or orbital textures in the Cr layer, governed by crystallographic orientation, may dominate angular momentum dissipation. The fourfold symmetry of magnetic damping is also observed in epitaxial CoFe films, but the smallest damping is along the in-plane easy axis, which is attributed to angle-dependent spin–orbit coupling rather than two-magnon–scattering processes.[38] Therefore, the origin of anisotropic magnetic damping in LSMO thin films requires further research to be clarified.

5.   Temperature-dependent damping
  • The temperature dependence of the FMR linewidth of sample A is presented in Fig. 4. The microwave absorption spectra were measured at various temperatures from 300 K to 5 K with a fixed frequency of 11 GHz, while all temperature-dependent measurements maintained an external magnetic field aligned along the [010]pc orientation of the LSMO thin films. Experimental measurements reveal a progressive broadening of the FMR linewidth in LSMO thin films as the temperature decreases from room temperature to cryogenic conditions, with the resonance linewidth ΔHpp estimated as 5 mT at 300 K, 10 mT at 150 K, and 20 mT at 5 K, as shown in Fig. 4(a). As the temperature decreases, the resonance absorption peak shifts toward higher magnetic fields, which can be attributed to changes in the saturation magnetization and magnetocrystalline anisotropy energy.[1]

    The epitaxial LSMO thin films (samples A, B, and C) were grown by slightly varying the laser energy density (0.64–0.65 J/cm2) while maintaining other growth conditions, with samples A and B prepared at higher energy density and sample C prepared at lower energy density. Distinct surface morphologies are revealed by atomic force microscopy (AFM) characterization, as shown in Fig. 4(b). Samples A and B exhibit similar granular topography with surface roughness values of Ra ∼ 0.974 and ∼ 0.890 nm, respectively. In contrast, sample C exhibits superior quality, characterized by atomic-scale terraces, with a remarkably low roughness of Ra ∼ 0.087 nm, which is approximately an order of magnitude smoother than both A and B. The magnetic damping constant α of samples A, B, and C was extracted by fitting the resonance linewidth ΔHpp and resonance frequency f under different temperatures, as shown in Fig. 4(c). All samples exhibit a non-monotonic damping curve, decreasing first and then increasing with decreasing temperature. A similar non-monotonic trend has also been observed in other LSMO films or heterostructures. In these reports, the temperature dependence of magnetic damping is considered to arise from contributions from spin pumping as well as resistivity-like (interband scattering) and conductivity-like (intraband scattering) mechanisms.[39,40] By contrast, the increased low-temperature magnetic damping in ferrimagnetic insulator YIG is explained by the impurity relaxation mechanism.[41]

    Interestingly, although the damping values of the three samples at room temperature are relatively close, they diverge significantly at low temperatures. The magnetic damping at 5 K of samples A, B, and C is 5.7 × 10−3, 7.4 × 10−3, and 2.5 × 10−3, respectively. The resonance linewidth of sample C at 5 K under 11 GHz is about 6 mT, which is significantly narrower than the 20 mT observed for sample A, as shown in Fig. 4(d). The half-metallic nature of LSMO/NGO thin films is confirmed by temperature-dependent resistivity, as shown in Fig. 4(e). The resistivity of sample C is 0.64 mΩ⋅cm at 300 K and 0.04 mΩ⋅cm at 4 K. The temperature dependence of magnetic damping in LSMO thin films is described by two terms, a resistivity-like part and a conductivity-like part, and their contributions are phenomenologically analyzed by the following model:

    where αρ and ασ represent the interband and intraband scattering parameters. ρ(T) and σ(T) are the temperature-dependent resistivity and conductivity of LSMO films. The fitting result of sample C is shown in Fig. 4(f). The parameter αρ for resistivity-like damping is ∼ 0.0018, and the parameter ασ for conductivity-like damping is ∼ 0.00013. For all samples, the suppression of magnetic damping with decreasing temperature is mainly attributed to the resistivity-like part, whereas the re-emergence below 150 K is primarily due to the conductivity-like part. The resistivity-like contribution to damping in all samples shows a similar trend, but the conductivity-like contribution exhibits a pronounced difference. As clearly seen in Figs. 4(a)–4(d), sample C with superior epitaxial quality demonstrates markedly reduced magnetic damping compared to samples A and B at low temperature. The improved epitaxial quality has significantly suppressed the contribution from the conductivity-like part associated with intraband scattering.

6.   Conclusion and perspectives
  • In summary, single-crystal epitaxial LSMO films with a thickness of 120 nm were successfully grown on NGO (110) substrates. The epitaxial quality and crystal structure were confirmed through surface topography and x-ray diffraction measurements. A fourfold symmetry of anisotropic magnetic damping was identified in the LSMO/NGO films, with a maximum-to-minimum ratio of approximately 150%. The half-metallic nature of LSMO films gives rise to a non-monotonic temperature dependence of magnetic damping. Importantly, we demonstrated that improving film quality effectively suppresses low-temperature magnetic damping by reducing intraband scattering. The highest-quality sample achieved a damping value of ∼ 2.5 × 10−3 at 5 K.

    These findings highlight an effective approach for tailoring cryogenic magnetic damping, paving the way for the exploration of quantum magnonic phenomena in manganites at low temperatures and expanding their potential applications in magnonic devices based on ferromagnet–superconductor heterostructures.

Figure (4)  Reference (41)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return