HTML
-
With the advancement of the electronics industry, the requirements for electronic materials are also increasing. Ceramics for lead-free dielectric energy storage have gained popularity as high-power density energy storage materials.[1–3] Various types of lead-free linear dielectric materials, ferroelectric materials, relaxor ferroelectric materials and antiferroelectric materials have been reported successively.[4,5] Recently, as electronic devices have been evolving towards miniaturization, integration and lightweight design, the demand for higher-performance energy storage components has been growing significantly. The high energy storage density of NaNbO3 (NN)-based relaxor ferroelectric ceramics enables them to store more energy in a smaller volume, which is beneficial for miniaturizing and enhancing the performance of electronic devices.[6–8] They can be applied to power management modules in portable electronic devices such as smartphones, tablets and laptops.
The following formulas can be used to determine the dielectric capacitors’ energy storage density and efficiency:[9,10]
Among them, Wtotal, Pm, Pr, Wrec, E and η represent total energy storage density, saturation polarization, residual polarization, recoverable energy storage density, electric field and efficiency, respectively.
The hysteresis loop of NN-based ceramics exhibits a square ferroelectric phase hysteresis loop, with significant residual polarization and limited energy storage performance (ESP). The polarization strength of linear dielectrics exhibits a linear relationship with the applied electric field, without hysteresis, thus achieving high energy storage efficiency.[11] Compared to the other types of ceramic capacitors, many linear dielectrics typically have a higher Eb.[12,13] However, extremely low polarization strength and dielectric constant severely limit their application in energy storage.[14–16] Therefore, by combining NN-based ceramics and linear dielectrics, the breakdown strength can be improved, residual polarization can be reduced and thus ESP can be enhanced. For instance, Feng et al.[17] added SrTiO3 (a linear perovskite material) into 0.76NaNbO3–0.24(Bi0.5Na0.5)TiO3 ceramics. At a 270 kV/cm of Eb, a Wrec of 2.64 J/cm3 and an ultra-high η of 89.9% were achieved. Kang et al.[18] investigated that the NaNbO3–Bi(Zn0.5Sn0.5)O3 added a linear dielectric material SrTiO3 (the added amount is 0.192), exhibited a Wrec of 5.82 J/cm3 and a η of 92.3%.[19]
In comparison to SrTiO3, CaTiO3 (CT) has a high dielectric strength (300 kV/cm) and a low dielectric loss (∼10−5).[20] In addition, its reported large band gap and dielectric constant are about 3.4 eV and 175, respectively.[21] These physical properties indicate that CT is a promising dielectric for enhancing the ESP of NaNbO3-based ceramics. Chen et al.[22] designed a (1 – x)(0.92NaNbO3–0.08Bi(Mg0.5Ti0.5)O3)–xCaTiO3 ceramic system, achieving a Wrec of 5.71 J/cm3 at 475 kV/cm with a 20% addition of CT. Zhang et al.[23] acquired a high Wrec of 6.84 J/cm3 in 0.6(0.96NaNbO3–0.04BiFeO3)–0.4CaTiO3. In our preliminary research, we obtained an Wrec of 3.2 J/cm3 in 0.7Na1–3xSmxNbO3–0.3(Sr0.7Bi0.2)(Ti0.8Zr0.2)O3 (abbreviated as xSm) ceramics, but its η was below 70%.[24] Therefore, by adding linear dielectric CT into 0.7Na1–3xSmxNbO3–0.3(Sr0.7Bi0.2)(Ti0.8Zr0.2)O3, we aim to improve its energy storage efficiency, which has never been studied.
-
The traditional solid-state sintering method was used to prepare (1 – x)[0.7Na0.97Sm0.01NbO3–0.3(Sr0.7Bi0.2)(Ti0.8Zr0.2)O3]–xCaTiO3 [abbreviated as xCT, x = 0.06, 0.09, 0.12, 0.15] ceramics. Sodium carbonate (Na2CO3, 99.8%), strontium carbonate (SrCO3, 99%), niobium pentoxide (Nb2O5, 99.9%), bismuth trioxide (Bi2O3, 99.8%), titanium dioxide (TiO2, 99%), zirconium dioxide (ZrO2, 99%), calcium carbonate (CaCO3, 99%) and samarium oxide (Sm2O3, 99.99%) were weighed in stoichiometric proportions and placed in a nylon ball mill jar. Zirconia balls were used as ball milling media and the mixture was subjected to ball milling with anhydrous ethanol for a duration of 8 h. Following the drying of the slurry, it was then calcined for 3 h at 950 °C in a muffle furnace. The resultant powder underwent a second ball milling for an additional 8 h. After drying, polyvinyl alcohol (PVA) was incorporated and the mixture was sieved through an 80 mesh sieve. The resulting product was compressed into a cylindrical green body at 200 MPa, and PVA was discharged at 600 °C for 2 h prior to sintering at 1240 °C–1300 °C for 2 h. Finally, the ceramic samples were polished to a thickness of approximately 0.1 mm, and then silver electrodes were applied to the surface to measure electrical performance.
Using the Archimedes method, the bulk density (ρbu) of the ceramics was determined. The relative density (ρre) was calculated as follows:
where ρth was the theoretical density and was obtained by the Rietveld refinement method. The phase structure of ceramic samples was investigated by x-ray diffraction (XRD, Ultima IV, Rigaku) and Raman spectroscopy (Raman, inVia Qontor, Renishaw). The microstructure was investigated through field-emission scanning electron microscopy (SEM, MIRA3, TESCAN), and the grain size was measured by means of Nano Measurer software. The dielectric performances were measured by a precision impedance analyzer (Impedance Analyzer E4990A, Keysight) in the temperature range of room temperature to 500 °C. The hysteresis loop (P–E) was tested via a ferroelectric testing system (TF Analyzer 2000 E, aixACCT). The charge–discharge performance was tested by a dielectric charge–discharge testing system (CFD-003).
-
The XRD patterns of xCT ceramics and the magnified (200) diffraction peaks are displayed in Fig. 1. As illustrated in Fig. 1(a), all ceramic components have a perovskite structure and no impurity phases are observed in the scanning range. This result indicates that CT has effectively infiltrated the NN lattice to form a solid solution. Figure 1(b) demonstrates that as the CT content rises, the diffraction peaks progressively shift towards higher angles, a phenomenon attributed to the lattice contraction of the ceramic, which results in a reduction of the unit cell volume. This is because the smaller ionic radius Ca2+ (1.34 Å, CN = 12) replaces the larger ionic radius Na+ (1.39 Å, CN = 12), Bi3+ (1.36 Å, CN = 12) and Sr2+ (1.44 Å, CN = 12). The (200) diffraction peaks of the ceramics split, showing a higher left side and a lower right side, demonstrating that the phase structure is orthorhombic.[25] The specific phase structure was determined by XRD Rietveld refinement.
In order to precisely characterize the changes in phase structure, GSAG software was used to fit the XRD data. Figure 2 indicates the refined patterns. Table 1 shows the refined parameters after fitting. The Rwp and Rp of all components are below 10%, and χ2 is between 1.370 and 1.569, demonstrating the reliability of Rietveld fitting. Moreover, the addition of CT significantly increases the content of AFE R phase, manifesting that CT is beneficial for improving the stability of AFE R phase. As the CT content increases, the R phase content gradually increases and remains predominant. However, the phase structure of the coexistence of AFE P and AFE R phases still exists in the xCT ceramics. In addition, the volume of the crystal cell gradually decreases, corroborating the previous XRD analysis results.
The density profiles of xCT ceramics are demonstrated in Fig. 3. All density curves initially experience a rise followed by a decline along with sintering temperature changes. High density (> 97.5%) is beneficial for improving dielectric and energy storage properties.
Figure 4 displays the Raman spectra of 0.7NaNbO3–0.3(Sr0.7Bi0.2)(Ti0.8Zr0.2)O3 [abbreviated as NN-SBTZ] and xCT ceramics, as well as the Gaussian–Lorentz function fitting curve at x = 0.06 (fitted using PeakFit software). In Fig. 4(a), as x increases, there is no significant change in the number of Raman peaks, implying that the phase structure of the ceramics remains stable. However, the peaks between 220 cm−1 and 600 cm−1 exhibit a gradual widening and flattening. This phenomenon is due to the enhancement of structural disorder and the weakening of cell polarity.[26] Compared with NN-SBTZ, the Raman curve of xCT ceramic shows the same trend before 700 cm−1, but there is an additional Raman peak at 1100 cm−1. One possible reason for this behavior is that the substitution of Sm3+ (1.24 Å) for Na+ (1.39 Å) in NaNbO3 can cause lattice contraction, resulting in shortened Nb–O bond length, enhanced bond energy, and a shift in vibration frequency towards higher wave numbers.[27,28] As a result, an additional Raman peak appears at 1100 cm−1.
Figure 5 shows the SEM images and relevant grain size distribution of xCT ceramics. The ceramic grains of all components are clearly visible, with distinct grain boundaries and no obvious pores. These findings imply that xCT ceramics, which are sintered at 1260 °C, possess a high density, a characteristic that is advantageous for enhancing ferroelectric properties. This is consistent with the test results in Fig. 3. The average grain sizes, as depicted in Figs. 5(a)–5(d), are measured as 3.78 μm, 3.35 μm, 3.28 μm and 3.21 μm for the samples with x values ranging from 0.06 to 0.15, respectively. Clearly, the average grain size of ceramics demonstrates a consistent decreasing trend. With the introduction of CT, the content of Bi gradually decreases. This decline in Bi concentration correlates with a decrease in the presence of oxygen vacancies, which subsequently inhibits the migration of grain boundaries and the growth of grains. Furthermore, this phenomenon may be attributed to the stochastic distribution of diverse A-site cations (Na+, Sm3+, Sr2+, Bi3+ and Ca2+), which contributes to an increase in lattice strain energy and further suppresses grain growth.[29] A smaller grain size is conducive to achieving high breakdown strength and improving Wrec.[30] In addition, the grain sizes of xCT ceramics are not uniform, as displayed in Fig. 5. This is because the ionic radius of Sm3+ (1.24 Å, CN = 12) is smaller than that of Na+ (1.39 Å, CN = 12). When Sm3+ is doped into NaNbO3, lattice distortion will be generated. Different degrees of local distortion may lead to a difference in diffusion rate, which in turn affects the grain growth rate. Figure 6 presents the energy dispersive spectroscopy (EDS) spectrum of 0.15CT ceramic, indicating a uniform distribution of elements, with their proportions aligning with theoretical values. This uniformity is advantageous for enhancing ESP.
Figure 7 illustrates the temperature-dependent dielectric constant (εr) and dielectric loss (tanδ) of xCT ceramics across various frequencies (1 kHz to 1 MHz). The εr of the ceramic gradually decreases with rising temperature, and no phase transition peak appears in any of the components. This means that xCT ceramics are mainly in the R phase at room temperature, with the phase transition point having dropped below room temperature.[31] None of the components exhibit a change in phase structure, and they are all coexisting two-phase structures, which is consistent with the previously mentioned XRD refinement results and Raman spectroscopy analysis results. As x increases, the εr gradually decreases. A larger εr will reduce the Eb of the ceramic, while a smaller εr will reduce the Pm of the ceramic. Therefore, this ceramic component of x = 0.15 is advantageous for obtaining higher Wrec due to its moderate εr. At temperatures above 350 °C, an increase in frequency for all ceramic compositions correlates with a decrease in tanδ. Furthermore, the tanδ of ceramics decreases as the doping amount increases at room temperature. Moreover, all the tanδ values at room temperature are below 1%. When x = 0.15, the dielectric loss of ceramics is the smallest, as shown in Fig. 7(e). Low tanδ is conducive to reducing energy loss and increasing η.
Figure 8 displays the εr and tanδ values for xCT ceramics tested at different frequencies. As x increases, the εr shows a decreasing trend. This is because the low polarized ion Ca2+ (polarization rate: Ca2+ = 3.16 × 10−3 nm3, Sm3+ = 4.74 × 10−3 nm3, Sr2+ = 4.25 × 10−3 nm3, Bi3+ = 6.12 × 10−3 nm3) reduces the polarization of A-site, and the polarity of B-site ions cannot compensate for the loss of A-site ion polarity, leading to a decline in εr. With the increase in frequency, the εr of ceramics remains basically unchanged. A medium dielectric constant can achieve high Pm and Eb values. When x = 0.15, it has an ultra-low tanδ (< 0.005), which is beneficial for reducing heat and achieving superior stability and high Eb value.
Figures 9(a)–9(c) show the unipolar polarization–electric field (P–E) loops of xCT ceramics at room temperature, as well as the corresponding variations of Pm, Pr, ΔP, Wrec and η with x. At x = 0.15, the ceramic demonstrates optimal ESP: Wrec = 3.9 J/cm3, η = 72.49%. Compared with the performance of 0CT ceramic (Wrec = 3.2 J/cm3, η = 69%), both Wrec and η are improved simultaneously when CT is added to the matrix, meeting the requirement of improving energy storage efficiency with linear dielectrics. The Eb is recognized as the critical determinant of ESP. To assess the Eb of xCT ceramics, the Weibull distribution analysis was employed, as depicted in Fig. 9(d). The relevant calculation formulas are provided as follows:[32,33]
where Xi and Yi represent variables in the Weibull expression, Ei denotes the breakdown strength, i represents the ordinal number and n signifies the total sample size (n = 8). The components of the Weibull index (β ≥ 10) have a linear relationship, indicating excellent reliability of Weibull distribution analysis.[34] Figure 9(d) shows that the breakdown strength reaches its maximum value at x = 0.15.
Figure 10 illustrates the unipolar P–E loops of 0.15CT ceramic under varying electric fields, as well as the corresponding changes in Pm, Pr, ΔP, Wrec and η. When the electric field increases to 470 kV/cm, Pm linearly increases to 20.89 μC/cm2, while Pr slowly increases to 2.66 μC/cm2, which also leads to a decrease in efficiency. Notably, Pm exhibits a significantly higher growth rate compared to Pr. This implies that as the electric field intensifies, the value of ΔP expands. Consequently, the change in Wrec is consistent with ΔP, with Wrec escalating to 3.9 J/cm3. However, the η declines slightly from 83.44% to 72.49%. This decrease in η is attributed to energy loss, which arises from the intensive residual polarization with the increase in electric field. One can deduce that for applications in high-electric-field environments, the optimal component should reduce residual polarization to achieve high η.
The excellent temperature/frequency stability of dielectric performance is a crucial parameter for maintaining the operational stability of ceramic capacitors. Figures 11(a)–11(c) illustrate the temperature/frequency-dependent unipolar P–E loops of 0.15CT ceramic at 200 kV/cm. Meanwhile, the relevant ESP, derived from Eqs. (1)–(3), is presented in Figs. 11(b) and 11(d), respectively. All samples exhibit slender P–E loops when measuring temperature and frequency. From Fig. 11(b), it can be observed that the increase in frequency has little effect on Wrec, with a change rate of only 0.5% to 0.7%, and has little effect on η, with a change rate of 3.38% to 5%. This analysis suggests that the ESP of 0.15CT ceramics is dependent on the stability of frequency (Wrec = 0.876 ± 0.005 J/cm3, η = 81.17% ± 3.02%). Similarly, from Fig. 11(d), the variation in amplitude of Wrec is very small within a wide temperature range (30 °C–120 °C), and the calculated change rate is only between 1.7% and 3.8%, with a slight decrease in η and a change rate between 2.5% and 3.64%. Therefore, the ESP of 0.15CT ceramic is temperature stable (Wrec = 0.916 ± 0.016 J/cm3, η = 74.84% ± 2.22%).
The underdamped and overdamped discharge current curves of 0.15CT ceramic at varying electric fields were characterized to identify its actual charge–discharge capacity. Current density (CD), power density (PD) and discharge energy density (Wd) are key performance parameters of capacitors in pulse charge–discharge performance, and the calculation formulas are as follows:[28,35]
where Imax represents the peak current, E stands for the magnitude of the electric field, S indicates the surface area of the silver electrode, R represents the load resistance and V represents the volume of the test sample. The fast charge–discharge characteristics of dielectric energy storage ceramics are also reflected in their short charge–discharge time. Short charge–discharge time means that ceramics can complete the charge–discharge process in a very short time, meeting the demand for fast response, represented by t0.9 (the value numerically corresponds to the discharge time at which Wd reaches 90% of its saturated state).
As depicted in Fig. 12(a), the peak current exhibits an increase with the electric field. At 12 kV/mm, the maximum discharge peak current is 10.25 A. As shown in Fig. 12(b), Imax, CD and PD at different electric fields show the same trend, steadily increasing with increasing electric field. Imax, CD and PD at 12 kV/mm reach 10.26 A, 326.4 A/cm2 and 39.17 MW/cm3, respectively. The overdamped discharge current of R = 200.5 Ω under varying electric fields is presented in Figs. 12(c) and 12(d). As the electric field intensifies, Wd increases to 0.8 J/cm3, with a charge–discharge rate of 27 ns, indicating superior charge–discharge speed relative to other studies.[24,29,35–40] This high charge–discharge rate renders the material particularly suitable for high-power and pulse power applications, including hybrid electric vehicles, medical defibrillators, spacecraft, satellites and electric weapon systems.
-
In this paper, xCT ceramics were prepared using the traditional solid-state reaction approach. The phase structure, microstructure, dielectric properties, energy storage and charge–discharge of ceramics were characterized. At an Eb of 470 kV/cm, 0.15CT ceramic achieves optimal ESP: Wrec = 3.9 J/cm3, η = 72.49%. Compared with 0.01Sm, Eb is significantly improved, ESP is enhanced and efficiency is promoted, meeting the requirements of using linear dielectrics to increase rates. In addition, 0.15CT ceramic also exhibits a PD of 39.17 MW/cm3, a CD of 326.4 A/cm2 and an extremely rapid charge–discharge rate, reaching 27 ns. The charge–discharge performance of this material surpasses that of 0.01Sm. Based on the above results, 0.15CT ceramic is a potential energy storage capacitor.
首页
登录
注册


DownLoad: