2026 Volume 35 Issue 5
Article Contents

Bo Sun, Yutong Zou, Tao Wang, Yujia Wang, Jinyu Liu, Lili Gao, Meiguang Zhang, Miao Zhang. Structural stability and mechanical properties of TiB6: A CALYPSO-guided exploration for superhard applications[J]. Chinese Physics B, 2026, 35(5): 056105. doi: 10.1088/1674-1056/adfb59
Citation: Bo Sun, Yutong Zou, Tao Wang, Yujia Wang, Jinyu Liu, Lili Gao, Meiguang Zhang, Miao Zhang. Structural stability and mechanical properties of TiB6: A CALYPSO-guided exploration for superhard applications[J]. Chinese Physics B, 2026, 35(5): 056105. doi: 10.1088/1674-1056/adfb59

Structural stability and mechanical properties of TiB6: A CALYPSO-guided exploration for superhard applications

  • Received Date: 15/06/2025
    Accepted Date: 20/07/2025
    Available Online: 01/05/2026
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(9)  /  Tables(2)

Article Metrics

Article views(258) PDF downloads(2) Cited by(0)

Access History

Structural stability and mechanical properties of TiB6: A CALYPSO-guided exploration for superhard applications

Abstract: Titanium–boron (Ti–B) compounds exhibit great promise as superhard materials due to titanium’s low atomic mass and abundant valence electrons. In this work, we systematically investigated the crystal structures of TiB6 under pressures ranging from 0–100 GPa using the CALYPSO algorithm combined with first-principles calculations. Phonon dispersion analysis and elastic-constant evaluations confirm the dynamic and mechanical stability of five predicted TiB6 structures. Notably, the α-Amm2-TiB6 structure was predicted to have a remarkable Vickers hardness of 56 GPa, as estimated by Chen’s empirical model. All five structures are thermodynamically stable under ambient conditions, suggesting viable synthetic pathways. Their outstanding bulk moduli and ultrahigh hardness further classify them as potential incompressible and superhard materials. These theoretical insights lay a robust foundation for future experimental synthesis efforts.

1.   Introduction
  • Superhard materials are extensively utilized in mechanical processing, aerospace, and various related areas owing to their exceptional mechanical properties.[1–3] The investigation of superhard materials exhibiting excellent properties is of fundamental significance for the advancement of condensed matter physics. Beyond the conventional superhard materials, such as diamond,[4] BC3,[5,6]c-BN,[7] and C3N2,[8] transition metal borides (TMBs) have attracted substantial interest on account of their high valence electron density and robust covalent bonds, superior wear resistance, and excellent oxidation resistance. These characteristics render them exceptional candidates for the development of new superhard materials.[9,10]

    To date, a number of TMBs have been experimentally synthesized or theoretically predicted.[11–25] For example, ReB2 was synthesized at ambient pressure with a Vickers hardness of 48 GPa.[11]Pnnm-CrB4 has been identified as a candidate for superhard materials, with its estimated Vickers hardness reaching 48 GPa.[12] Nevertheless, the experimentally measured Vickers hardness is only 23.3 GPa.[26] Both phases of WB4 exhibit a high bulk modulus, a high shear modulus, and a low Poisson’s ratio, making WB4 a promising material with low compressibility.[27] Moreover, WB4 has demonstrated an outstanding combination of high strength and improved ductility under shear strain.[28] Recent theoretical investigations have indicated that ZrB6 can be synthesized experimentally at moderate pressures, achieving a Vickers hardness > 40 GPa.[13] The recently predicted structure C2-HfB6 is expected to exhibit a superhardness of up to 50 GPa, positioning it as a potential superhard material.[14] The Amm2-TaB6 phase demonstrates a high bulk modulus and strong resistance to compression, with a Vickers hardness of 40.8 GPa.[15] Notably, most TMBs contain transition metal elements that are heavier than titanium. Due to its relatively lighter atomic mass and abundant valence electrons, titanium-based systems may facilitate synthesis. A variety of Ti–B compounds have been synthesized, including TiB, TiB2, and Ti3B4.[29,30] In theoretical work, Ti3B4, Ti2B3, TiB2, Ti2B5, TiB3, TiB4, and TiB12 have been identified as potential superhard materials,[31–36] exhibiting simulated hardness values ranging from 32.3 GPa to 53.3 GPa. In particular, Amm2-TiB3 exhibits a hardness value of 51.6 GPa,[33] while Cmcm-TiB4 demonstrates a hardness value of 53.3 GPa.[34] The remarkable hardness of TiB3 and TiB4 motivates systematic investigation of novel boron-rich Ti–B compounds as potential candidates for superhard materials.

    Within this study, we comprehensively explore the crystal structure and properties of TiB6 via the CALYPSO method combined with first-principles calculations. Utilizing Chen’s model, we predict five novel phases: α-Amm2, β-Amm2, P2/m, α-P21/m, and β-P21/m. Among the proposed structures, the Vickers hardness of α-Amm2-TiB6 reaches 56 GPa, rendering it the hardest titanium-boron compound identified to date. Computational analyses indicate that the five structures exhibit both dynamical and thermodynamic stability at atmospheric pressure. This research contributes to the ongoing exploration of new superhard materials.

2.   Methods
  • Density functional theory (DFT), implemented in the Vienna ab initio simulation package (VASP), was employed to conduct structural optimization and electronic structure calculations.[37,38] We explored the properties of TiB6 in the pressure range of 0–100 GPa using the CALYPSO code,[39] which has been specifically designed to explore the potential energy surfaces of chemical systems and identify global minima.[40] The electron exchange–correlation interactions were described using the generalized gradient approximation (GGA) formulated by Perdew, Burke, and Ernzerhof (PBE).[41,42] The projector augmented-wave (PAW)[43] method was used to treat ion–electron interactions, explicitly considering the 2s22p1 electrons of B atoms and the 3s23p64s23d2 electrons of Ti atoms.[44] To ensure accuracy, a plane-wave energy cutoff of 800 eV was used. Furthermore, dense Monkhorst–Pack k-meshes[45] of 10 × 16 × 8 for α-Amm2, 10 × 16 × 4 for β-Amm2, 11 × 17 × 6 for P2/m, 7 × 18 × 12 for α-P21/m, and 17 × 18 × 5 for β-P21/m were used. Phonon dispersion curves were calculated using a supercell approach implemented in the PHONOPY code to assess dynamical stability.[46] Elastic constants were derived using the strain–stress method. Subsequently, bulk modulus, shear modulus, Young’s modulus, and Poisson’s ratio were computed via the Voigt–Reuss–Hill approximation. Vickers hardness values were evaluated using Chen’s model[47] and Tian’s model.[48]

3.   Results and discussion
  • We employed the CALYPSO method combined with first-principles calculations to explore stable TiB6 compounds. We propose two orthorhombic phases: α-Amm2 and β-Amm2, along with three monoclinic phases: P2/m, α-P21/m, and β-P21/m, as illustrated in Fig. 1. For α-Amm2-TiB6 and β-Amm2-TiB6, each Ti atom is surrounded by twelve neighboring B atoms. The B atoms form parallel hexagonal planes with misaligned stacking arrangements. The B–B bonds exhibit bond lengths ranging from 1.72 Å to 1.83 Å. Importantly, the shortest B–B bonds in the predicted α-Amm2-TiB6 and β-Amm2-TiB6 phases are substantially shorter than those observed in established hard materials such as OsB2 (1.85 Å).[49] Ti atoms are located at the central positions of two six-membered boron rings, and these rings differ in the number of boron layers. The α-Amm2 structure contains three layers, while the β-Amm2 structure consists of five layers. P2/m, α-P21/m, and β-P21/m exhibit layered stacking along the b-axis, and Ti atoms occupy similar central positions within boron frameworks. The B–B bonds exhibit bond lengths ranging from 1.53 Å to 1.78 Å. The lattice constants, cell volumes, and atomic positions of TiB6 after relaxation are listed in Table S1.

  • Here, we report the enthalpy differences of β-Amm2-TiB6, P2/m-TiB6, α-P21/m-TiB6, and β-P21/m-TiB6 relative to the α-Amm2-TiB6 phase as a function of pressure. We also present information on metastable titanium borides at 0 GPa, 50 GPa, and 100 GPa. As shown in Fig. 2(a), the calculated enthalpy curves reveal the pressure ranges where different phases are thermodynamically stable. Up to 13 GPa, the α-P2/m phase becomes more stable. When the pressure reaches 28 GPa, α-Amm2-TiB6 becomes energetically favorable, and then transforms to β-Amm2- and β-P21/m-TiB6 at 31 GPa and 62 GPa, respectively. Figures 2(b)–2(d) illustrate the thermodynamic convex hull of the Ti–B system, indicating that Pnma-TiB, P6/mmm-TiB2,[50] and Immm-Ti3B4 are thermodynamically stable titanium borides at ambient pressure. The predicted TiB6 compounds are metastable at ambient conditions. As shown in Figs. 2(b)–2(d), the formation enthalpy decreases with increasing pressure, reaching its minimum at 100 GPa. This suggests that the metastable TiB6 phases may become stabilized under high pressure.

    In order to demonstrate the dynamical stability of TiB6, we assessed the lattice dynamics of the five structures by calculating their phonon spectra. Typically, the absence of imaginary phonon modes confirms dynamical stability.[51–53] As depicted in Fig. 3, the phonon dispersion relations of the TiB6 compounds at atmospheric pressure exhibit no imaginary frequencies within the Brillouin zone. Notably, the α-Amm2 phase maintains a stable phonon spectrum even at 30 GPa, which coincides with its thermodynamic stability range (28–31 GPa). These results confirm that all predicted TiB6 structures are dynamically stable under ambient pressure conditions.

    To evaluate the thermodynamic stability of the TiB6 phases, we systematically determined the pressure-dependent formation enthalpies through four distinct synthetic pathways, as illustrated in Figs. 4 and S1. In the range of 0–100 GPa, with increasing pressure, the formation enthalpy becomes more negative, indicating that pressure enhances structural stability. The formation enthalpies of TiB6, defined by Eqs. (1)–(4), are calculated with respect to distinct reference phases (including elemental Ti/B, TiB, Ti3B4, and TiB2) to comprehensively evaluate its thermodynamic stability.

    The P6/mmm-Ti, P6/mmm-TiB2,[50]α-B, and γ-B[54] are chosen as reference phases. As illustrated in Fig. 4, various reaction pathways were identified based on different synthesis conditions. Here, taking the α-Amm2 and β-Amm2 phases of TiB6 as examples, the fourth reaction pathway involving TiB2 as a precursor is not accessible within the pressure range of 0–100 GPa. In contrast, the first and second pathways with negative formation enthalpies are thermodynamically favorable. The third pathway becomes accessible under conditions of 6.8 GPa and 7.8 GPa for the two structures, respectively. These results indicate that the five predicted TiB6 phases are thermodynamically stable at ambient conditions.

  • Besides evaluating thermodynamic and dynamical stability, we additionally assessed the mechanical stability of the predicted structures. The mechanical stability of the phases is determined via the analysis of elastic constants (Cij).[55] For the orthorhombic and monoclinic crystal systems considered in this study, the mechanical stability criteria require that the elastic constants satisfy specific constraints. Orthorhombic lattices must adhere to the following conditions.

    For orthorhombic crystals,[56]

    For monoclinic crystals,[56]

    As presented in Table 1, the elastic constants of all TiB6 structures under investigation satisfy the mechanical stability criteria, thereby confirming their mechanical stability under ambient pressure conditions. To provide a reference for comparative analysis with the newly predicted structures, the corresponding data of previously reported C2/m-Ti2B5,[36]Amm2-TiB3,[33]C2/m-TiB3,[33]Amm2-TaB6,[15] and Amm2-HfB6[18] at 0 GPa were also listed in Table 1. All structures exhibit significantly large values of C11, C22, and C33, indicating that compression along the a-, b-, and c-axes is difficult, respectively. Of particular note is α-Amm2-TiB6, where C11 = 694 GPa and C22 = 663 GPa, indicating its extreme incompressibility along the a- and b-axes. Collectively, all TiB6 phases demonstrate thermodynamic, dynamical, and mechanical stability at 0 GPa.

    The Voigt–Reuss–Hill approximation was employed to derive the bulk modulus (B) and shear modulus (G) from the elastic constants. Young’s modulus (E) and Poisson’s ratio (ν) were subsequently calculated using the standard relations E = 9BG/(3B + G) and ν = (3B – 2G)/(6B + 2G), respectively. These parameters, including B, G, E, and ν, are systematically tabulated in Table 2. The estimated hardness of the five TiB6 compounds was evaluated using Chen’s model: HV = (2k2G)0.585–3 and Tian’s model: HV = 0.92k1.137G0.708–3, where Pugh’s ratio is denoted by k and G is the shear modulus. The computed hardness values are also listed in Table 2.

    Significantly, the orthorhombic α-Amm2-TiB6 phase demonstrates exceptional mechanical performance, achieving a theoretical hardness of 55.9 GPa. This value not only exceeds previous records within the Ti–B system, but also surpasses the hardness of previously reported transition-metal boride compounds. These findings provide important theoretical insights for the rational design of novel transition-metal boride superhard materials. Furthermore, the calculated shear modulus (G) and Vickers hardness of C2/m-Ti2B5,[36]Amm2-TiB3,[33]C2/m-TiB3,[33]Amm2-TaB6,[15] and Amm2-HfB6[18] at ambient pressure were also listed in Table 2, together with comparative data from previous studies. These results are consistent with previous theoretical predictions for transition-metal borides, thus validating the reliability of the computational approach.

    Elastic anisotropy in crystals exhibits orientation dependence. To visually demonstrate elastic anisotropy, the variations of the bulk modulus and Young’s modulus with crystal orientation were investigated.[57,58] For isotropic crystals, three-dimensional (3D) plots of elastic parameters should exhibit spherical symmetry, and any deviation from sphericity indicates elastic anisotropy. Taking the α-Amm2 and β-Amm2 phases of TiB6 as examples, Figs. 5(a) and 5(c) display the 3D plots of the bulk modulus and Young’s modulus of α-Amm2-TiB6. The 3D plots of α-Amm2-TiB6 are not spherical. More pronounced anisotropy is observed in Young’s modulus compared with the bulk modulus. The calculated ratios of Bmax/Bmin and Emax/Emin are 1.195 and 1.295, respectively, indicating anisotropic elastic behavior. Figures 5(b) and 5(d) display two-dimensional (2D) projections of bulk modulus and Young’s modulus for α-Amm2-TiB6 on the xy, xz, and yz planes. These projections demonstrate the directional dependence of elastic properties, revealing the anisotropy of α-Amm2-TiB6. In particular, the 2D projection of the bulk modulus on the xy plane is nearly circular. In contrast, elastic anisotropy is significant on the xz and yz planes, where the projection curves are noncircular. Likewise, the elastic anisotropy of β-Amm2-TiB6 is investigated through 3D renderings of bulk modulus and Young’s modulus, illustrated in Figs. 6(a) and 6(c). Specifically, Young’s modulus exhibits pronounced anisotropy. This feature originates from the deviation of its 3D surface from spherical symmetry, indicating direction-dependent deformation resistance. The 3D plots of β -Amm2-TiB6 are not spherical. Again, compared with the bulk modulus, Young’s modulus shows more obvious anisotropy. The calculated ratios of Bmax/Bmin and Emax/Emin are 1.233 and 1.299, respectively, indicating anisotropic elastic behavior. The 2D projections in Figs. 6(b) and 6(d) further support this conclusion. Since α-Amm2-TiB6 and β-Amm2-TiB6 have similar structures, differing only in the number of B layers, they exhibit nearly identical anisotropy. 3D plots and 2D projections of bulk modulus and Young’s modulus for the three monoclinic structures are illustrated in Figs.S4–S6. From the above analysis, the following conclusions can be drawn. (I) Elastic isotropy is approximately observed for the bulk modulus in the xy plane. (II) The anisotropy of Young’s modulus in the xy plane is weaker than that in the xz and yz planes. (III) Both materials exhibit relatively strong anisotropy in Young’s modulus.

  • In order to further investigate the electronic properties of TiB6 phases at ambient pressure, we performed a comprehensive analysis of their band structures, as illustrated in Fig. 7. The results show that all TiB6 phases exhibit multiple electronic bands crossing the Fermi level, accompanied by a finite density of states at the Fermi energy. These features confirm the metallic behavior of these borides and suggest potential electrical conductivity.

    To gain a better understanding of the electronic properties of TiB6, we calculated the projected densities of states (PDOS) of the α-Amm2 and β-Amm2 phases, as shown in Fig. 8. The PDOS analysis reveals that the Ti-3d and B-2p orbitals play dominant roles in their metallicity. The metallic behavior in all investigated compounds originates from the non-zero density of states at the Fermi level. States below −5 eV are predominantly derived from B-2s and B-2p orbitals, while contributions in the −5 eV to 0 eV range mainly arise from hybridization between B-2p and Ti-3d states. Notably, the B-2s states are partially hybridized with B-2p states, leading to strong localization within the boron sublattice. This hybridization facilitates the formation of robust covalent B–B bonds, which significantly enhance deformation resistance and intrinsic hardness of TiB6. In addition, distinct orbital hybridization occurs between Ti-3d states and B-2s or B-2p states. This localized Ti–B orbital hybridization drives the formation of directional Ti–B bonds. Consequently, the exceptional hardness of TiB6 arises synergistically from two key factors: the covalent bonding network within the B–B framework and the directional covalent bonding between Ti and B atoms. This analysis is consistent with fundamental principles of electronic structure in transition-metal borides, where hybridization between metal d orbitals and light-element p orbitals governs macroscopic mechanical properties. The PDOS results for the monoclinic phases are presented in Supplementary Fig. S3.

    To gain deeper insights into the bonding characteristics of TiB6, we performed electronic localization function (ELF) calculations to analyze electron pairing. In Fig. 9, the ELF contour distributions of α-Amm2-TiB6 on the (001) plane are presented, while those for β-Amm2-TiB6 are shown on the (1¯00) plane at 0 GPa, with additional monoclinic data provided in Fig. S2. The analysis demonstrates that significant electron localization exists between neighboring B atoms. Such covalent bonding features directly contribute to the enhanced mechanical hardness and structural integrity of the TiB6 system, as evidenced by the robust electron localization patterns. These results establish the critical role of B–B covalent bonding in determining the mechanical properties.

4.   Conclusion
  • In conclusion, to investigate novel transition-metal boride superhard materials, we employed the CALYPSO algorithm combined with first-principles calculations to predict the crystal structures of TiB6. Our analysis yielded five stable phases: α-Amm2, β-Amm2, P2/m, α-P21/m, and β-P21/m. Notably, the α-Amm2-TiB6 phase exhibits exceptional hardness. According to Chen’s model, its Vickers hardness is estimated to reach 55.9 GPa, indicating its potential as a superhard material. Compared with previously reported TiB compounds, the newly proposed α-Amm2-TiB6 is among the hardest known phases in the Ti–B system. The stability of all explored TiB6 compounds, including dynamical, thermodynamic, and mechanical stability, was confirmed through phonon spectra, formation enthalpies, and elastic constant calculations.

Figure (9)  Table (2) Reference (58)