2025 Volume 34 Issue 11
Article Contents

Liangrui Tan, Donglin He, Zhibiao Xu, Guowu Wang, Shengyu Yang, Shaoyong Leng, Ruilong Li, Tao Wang. High-frequency complex permeability calculation for metallic soft magnetic particles with easy magnetization plane in non-magnetic medium[J]. Chinese Physics B, 2025, 34(11): 117501. doi: 10.1088/1674-1056/ae00ad
Citation: Liangrui Tan, Donglin He, Zhibiao Xu, Guowu Wang, Shengyu Yang, Shaoyong Leng, Ruilong Li, Tao Wang. High-frequency complex permeability calculation for metallic soft magnetic particles with easy magnetization plane in non-magnetic medium[J]. Chinese Physics B, 2025, 34(11): 117501. doi: 10.1088/1674-1056/ae00ad

High-frequency complex permeability calculation for metallic soft magnetic particles with easy magnetization plane in non-magnetic medium

  • Received Date: 04/06/2025
    Accepted Date: 30/07/2025
    Available Online: 01/11/2025
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(6)

Article Metrics

Article views(480) PDF downloads(3) Cited by(0)

Access History

High-frequency complex permeability calculation for metallic soft magnetic particles with easy magnetization plane in non-magnetic medium

Abstract: Soft magnetic composites made from metallic magnetic particles with an easy magnetization plane (referred to as easy-plane metallic soft magnetic composites (SMC)) are considered ideal materials for the next generation of power electronic devices. This advantage is attributed to their ability to maintain high permeability at elevated frequencies. Despite these advantages, a definitive mathematical model that connects the high-frequency magnetic properties (e.g., effective permeability) of easy-plane metallic SMCs to the intrinsic properties of the particles is still lacking. In this work, a theoretical calculation model for the effective permeability of easy-plane metallic SMCs was formulated. This model was derived from a skin effect-corrected Landau–Lifshitz–Gilbert (LLG) equation and integrated with effective medium theory incorporating inter-particle interaction. To validate the model, we prepared samples of easy-plane Y2Co17 particle/PU SMCs with varying particle sizes and volume fractions. The experimental results showed a strong agreement with the calculated values. This research offers critical theoretical backing for the design and optimization of soft magnetic materials intended for high-frequency applications.

1.   Introduction
  • Metallic soft magnetic composites (SMCs), composed of metallic magnetic particles and insulating binders, blend the benefits of high resistivity and saturation magnetization. They find widespread applications in energy transmission and conversion–such as power inductors,[1–6] microwave absorption,[7–9] and information technology, including communication antennas.[10–13] As power electronics and information technology advance, the trend toward miniaturization and high-frequency operation in energy devices, absorbers, and antennas is evident. The demand for high-performance metallic SMCs that sustain high permeability at elevated frequencies is pressing. The efficacy of metallic SMCs hinges on the intrinsic properties of metallic magnetic particles. Studies reveal that metallic magnetic particles with an easy magnetization plane (easy-plane particles) outperform traditional counterparts at higher frequencies.[14–20] Therefore, establishing a theoretical model that links the intrinsic parameters of easy-plane particles (e.g., size, electrical resistivity, saturation magnetization) to the effective permeability of SMCs composed of these particles (easy-plane metallic SMCs) is crucial for optimizing their high-frequency performance.

    Recent efforts have delved into the complex permeability characteristics of metallic SMCs.[21–32] Wu et al.[33] explored the distribution of particle magnetic moments and effectively determined the permeability of SMCs containing spherical iron particles using effective medium theory. However, their study relied on the conventional Landau–Lifshitz–Gilbert (LLG) equation, rendering it unsuitable for easy-plane metallic SMCs, which exhibit greater potential in high-frequency applications. Additionally, the study’s approach to particle magnetic moment orientation had limitations, failing to account for arbitrary magnetic moment orientations and unable to predict the effective permeability of SMCs at high particle loadings. While scholars like Li et al.[34] acknowledged the benefits of easy-plane particles and proposed a bi-anisotropic model using the LLG equation to calculate the susceptibility of easy-plane metallic SMCs, this model still has critical limitations, as it inadequately accounts for interparticle interactions and applies only to scenarios with uniformly distributed magnetic moments.

    In response to these challenges, this study aims to develop a theoretical calculation model for the effective permeability of easy-plane metallic SMCs. This model is composed of two parts: an intrinsic permeability calculation model for easy-plane particles and an effective permeability calculation model tailored to easy-plane metallic SMCs. The model addresses skin effect corrections and the impact of high particle volume fractions. To validate the model, we prepared samples of easy-plane Y2Co17/PU SMCs with varying particle sizes and volume fractions.

2.   Algorithm details
  • Figure 1 illustrates the flowchart detailing our algorithm. We utilized the LLG equation, tailored for easy-plane systems, to calculate the intrinsic permeability of a single easy-plane metallic magnetic particle based on material-specific intrinsic parameters. Subsequently, we considered the magnetic moment distributions of multiple particles to determine the ensemble-averaged permeability. In this step, we employed effective medium theory to determine the effective permeability of easy-plane particle-based SMCs. Notably, our calculations incorporate the particle size effects to accurately account for skin effects.

  • The magnetization M of the magnetic particles is described by the LLG equation[35]

    Here, γ represents the gyromagnetic ratio, α is the Gilbert damping factor, and Ms denotes the saturation magnetization of the particles. The total effective field Heff = Ha + h includes the static magnetic field Ha and the microwave field h.

    Considering the easy-plane nature of the particles, the total effective field Heff can be expressed as[15]

    Here, H⊥ and H∥ denote the out-of-plane and in-plane anisotropy fields, Mi (i = 1,2,3) represent the components of the magnetization M along the principal axes 1, 2, and 3, and hi (i = 1,2,3) represent the components of the microwave field h along these axes.

    By substituting Heff into the LLG equation, we derive

    Here

    It is important to note that all the above derivations are performed in the particle’s principal axis coordinate system o-123. For practical calculations, coordinate transformation is essential to harmonize the results into the laboratory coordinate system. After transformation, the intrinsic permeability of the easy-plane particle is given by[34]

    Here

    where θ, ϕ, and δ represent the directional angles of the particle’s magnetic moment, while θh and φh denote the polar and azimuthal angles of the microwave field in the spherical coordinate system.

  • The metallic SMC consists of numerous metallic magnetic powder particles, each of which contributes to the overall permeability. The permeability of an individual particle is influenced by the angle between the microwave field and its magnetic moment. To accurately calculate the effective permeability of the SMC, the collective influence of all particles in the ensemble must be considered to derive the ensemble-averaged permeability. The intrinsic permeability of a single particle is calculated using Eq. (5), and the ensemble-averaged permeability can be written as

    Here, μi(θ, φ) represents the intrinsic permeability of an individual particle, and N denotes the total number of particles in the simulation.

  • Traditionally, the magnetic moment distribution of oriented samples has been simulated using a Gaussian distribution. However, the parameters of the Gaussian distribution cannot be directly correlated with physical quantities, thus lacking physical significance. To address this limitation, we propose a magnetic moment distribution model based on the Boltzmann distribution, which establishes the relationship between the orienting magnetic field and the orientation degree of the sample.

    The orientation of magnetic moments in magnetic particles within a rotating magnetic field is governed by the interplay between thermodynamic equilibrium and the applied magnetic field. According to the Boltzmann distribution in statistical mechanics, the energy E of a magnetic moment m under the applied magnetic field H is given by

    Here, m = |m| represents the magnitude of the magnetic moment, H = |H| denotes the strength of the applied magnetic field, and θ is the angle between the magnetic moment and the magnetic field. Owing to the rotational symmetry of the system, the probability density function depends only on the polar angle θ and is independent of the azimuthal angle φ. By incorporating the Boltzmann distribution, the probability density function for the oriented magnetic moment is expressed as

    Here, kB is the Boltzmann constant, and T is the absolute temperature. The partition function Z is defined as Z=∫02π∫0πemHcos(θ)kBTsin(θ)dθdφ. For convenience, the probability density function is written as

    Here, ξ=mHkBT is a dimensionless parameter characterizing the relative interaction strength between the magnetic moment and the external field. To simulate the distribution of magnetic moments with different orientations, we employ the inverse transform sampling method, which generates random samples from a known cumulative distribution function (CDF).

    The CDF for the oriented magnetic moment is expressed as

    Since P(θ) is the probability density function (PDF) and F(θ) is the corresponding CDF over the interval [0,1], the inverse cumulative distribution function (ICDF) is defined as the inverse of the CDF

    For any probability u ∈ [0,1], F−1(u) returns an angle θ such that F(θ) = u. In practice, direct sampling from the target distribution can be challenging; instead, uniformly distributed random numbers u are generated and transformed into samples x from the target distribution using the ICDF. Due to the typically complex nature of the ICDF, which is often not analytically solvable, we exploit the monotonicity of the CDF to numerically approximate the ICDF via interpolation, thereby improving computational efficiency.

    The orientation degree D is defined as the percentage of magnetic moments distributed within a small angle around the xy-plane relative to the total number of magnetic moments, ranging from 0 to 100. Specifically, the orientation degree D is evaluated as

    Here, M is the total number of magnetic moments, and Mxy denotes the number of magnetic moments distributed within a small angle around the xy-plane.

    Figures 2(a)–2(d) depict the simulation results of magnetic moment distributions at different orientation degrees. In these figures, red dots indicate the centers of unit spheres (radius = 1), while points on the sphere surfaces correspond to the simulated magnetic moment distributions. Vectors extending from the red dots to the surface points indicate the directions of the magnetic moments. Figure 2(e) shows the probability histogram of the magnetic moment distribution across different orientation degrees. For the samples prepared in this study, the random distribution pattern shown in Fig. 2(a) is relevant. A total of 10000 magnetic moments were considered when computing the ensemble-averaged intrinsic permeability of the particles.

  • SMCs can be regarded as systems in which magnetic particles are embedded within a non-magnetic insulating matrix. In such setups, the effective permeability is commonly calculated using effective medium theory (EMT). A commonly used approach is the Bruggeman effective medium theory, formulated as[36,37]

    Here, f1 represents the volume fraction of magnetic particles, μ1 denotes the average permeability of the particle ensemble, μ2 signifies the permeability of the matrix (with μ2 = 1 for non-magnetic matrices), and μeff stands for the effective permeability of the composite.

    Although the Bruggeman effective medium theory primarily accounts for mean-field effects, its accuracy decreases at high volume fractions. Yin et al.[22] incorporated pairwise particle interactions and employed the Green’s function method to solve the local magnetic field. By averaging the local field results, they developed a more accurate effective permeability model, particularly suitable for high-volume fractions and complex microstructures, referred to here as the HEMT. The HEMT is expressed as

    Here, α=3μ0μ1+2μ0, β=μ1−μ0μ1+2μ0, ϕ is the volume fraction of magnetic particles, μ1 denotes the average permeability of the particle ensemble, μ0 represents the permeability of the matrix (with μ0 = 1 for non-magnetic matrices), and μeff is the effective permeability of the composite. In this work, the effective permeability of the composite is calculated using the HEMT.

  • The skin effect inevitably arises in metallic soft magnetic particles under high-frequency microwave fields. Comsol was employed to simulate the distribution of magnetic field intensity H inside an iron sphere with a radius of 1 μm under a 400 A/m microwave magnetic field. Figures 3(a)–3(d) correspond to the simulation results at microwave magnetic field frequencies of 1 MHz, 10 MHz, 100 MHz, and 1 GHz, respectively. The simulation results show that the magnetic field intensity decays rapidly within the particle and is confined to a surface layer, with this effect becoming more pronounced at higher microwave frequencies. Therefore, it is vital to incorporate skin effect corrections into the calculations.

    An alternating microwave magnetic field h0 propagates along the Z-axis into the material, and the microwave field h inside the material can be represented as

    Here, ω denotes the angular frequency of the microwave. e−z/δ is the attenuation factor, where δ stands for the skin depth given by δ=ρπμif, with ρ representing the resistivity, μi the intrinsic permeability, and f the microwave frequency. The microwave field gradually attenuates as it penetrates deeper into the material. For spherical particles, the microwave field inside the particle can be expressed as[33]

    where R represents the particle radius. The particle’s dynamic magnetization is expressed as

    Here, χi denotes the intrinsic magnetization of the particle. Consequently, the intrinsic permeability of a single particle, including the skin effect, is given by

    The average permeability of the particle ensemble, accounting for the skin effect, is calculated as

    The effective permeability of the metallic SMC, incorporating the skin effect into the HEMT model, is given by

    Here, 〈α〉fix=3μ0〈μ〉fix+2μ0, 〈β〉fix=〈μ〉fix−μ0〈μ〉fix+2μ0.

3.   Experiment details
  • The Y2Co17 alloy, which resembles Co2Z and exhibits high saturation magnetization, is a prototypical easy-plane metallic soft magnetic material, with magnetization preferentially aligning within the c-crystal plane. This material was chosen to validate the algorithm presented in this work.[38] A series of composite samples containing Y2Co17 powders with varying particle sizes and volume fractions were fabricated, and their complex permeabilities were measured experimentally. The efficacy of the proposed algorithm was confirmed through a comparison between calculated results and experimental data.

    The Y2Co17 alloy was prepared by the vacuum induction melting method. The resulting alloy ingot was crushed, ground, and sieved to obtain powders with particle sizes of 100–200 mesh and 400–500 mesh. The powder within the 100–200 mesh category was labeled as BD powder, while the 400–500 mesh Y2Co17 powder underwent ball milling to become SD powder. Ball milling was conducted using 6 mm zirconia balls in n-heptane, with a ball-to-powder ratio of 20:1, at a rotation speed of 200 rpm for 2 hours. To formulate the composites, polyurethane (PU) was used as a binding agent. Oriented samples (used to verify the easy-plane property of Y2Co17) were prepared by a rotating magnetic field orientation method. For non-oriented samples, the dried SD/BD powders coated with PU were pressed into discs (15 mm in diameter) under a pressure of 340 MPa (approximately 6 tons). The discs were then stamped into toroidal rings (outer diameter = 7 mm, inner diameter = 3 mm) for permeability measurements.

  • The Y2Co17 powder was analyzed by x-ray diffraction (XRD, Philips, Cu-Kα radiation). The morphology of the powders with different particle sizes was examined using scanning electron microscopy (SEM, Thermo Fisher Scientific Apreo S4800). Permeability was measured at room temperature in the frequency range of 1 MHz to 1 GHz using an impedance analyzer (Agilent E4991B), and in the frequency range of 100 MHz to 18 GHz using a vector network analyzer (Agilent Technologies PNA-X N5247A). The hysteresis loop was obtained using a vibrating sample magnetometer (Lake Shore EV9). To acquire the in-plane and out-of-plane initial magnetization curves for the oriented samples, a superconducting quantum interference device (Quantum Design SQUID-VSM) was utilized.

4.   Results and discussion
  • SEM images of the BD and SD powders are depicted in Figs. 4(a) and 4(b), respectively, unveiling the irregular block-like morphology of the powder particles. Analysis of particle sizes reveals an average size of approximately 120 μm for BD powder and about 5 μm for SD powder. The hysteresis loop illustrated in Fig. 4(c) indicates a saturation magnetization of 132 emu/g and a coercivity of 50 Oe for the Y2Co17 powder, consistent with previous reports.[39] Figure 4(d) presents the XRD pattern of the Y2Co17 powder, displaying good consistency with the standard powder diffraction file card (PDF#97-062-5583), thus confirming the purity of the prepared sample.

    To verify the easy-plane property of Y2Co17 and measure the out-of-plane anisotropy field of the SMC, oriented SD/PU composite samples were created. Figure 4(e) illustrates the XRD pattern of the oriented SD/PU composite. Compared with the non-oriented sample, the intensity of the (006) crystal plane peak of oriented Y2Co17 was significantly increased, indicating the alignment of easy magnetization planes of particles parallel to the applied orientation magnetic field. Figure 4(f) depicts the normalized in-plane and out-of-plane initial magnetization curves for the oriented SD/PU composite, highlighting the substantial anisotropy induced by the orientation treatment. Figures 4(e)–4(f) clearly indicate the easy-plane property of Y2Co17.

  • In essence, Ms, H⊥, H∥ and a are crucial parameters for calculating the complex permeability of SMCs. As shown in Fig. 4(c), Ms ≈ 1.1 × 106 A/m (about 132 emu/g). The out-of-plane anisotropy field H⊥ is determined as the intersection field of the in-plane and out-of-plane initial magnetization curves for the oriented SMC,[40] as depicted in Fig. 4(f), where H⊥ ≈ 2.4 × 106 A/m (roughly 3 T). To extract the in-plane anisotropy field H∥, a low-fill sample with a 35% volume fraction was chosen due to its weak interparticle interaction effect. Figure 5(a) displays the permeability of the 35% volume fraction SD powder composite, exhibiting a natural resonance frequency fr = 5.5 GHz, consistent with the natural resonance frequency formulation for easy-plane systems[15,34]

    The corresponding value of H∥ ≈ 1.01 × 104 A/m. Our experimental results indicate that a damping coefficient of a = 0.6 provides good agreement between experimental and theoretical data.

    Various SMCs with volume fractions of 10%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, and 60% were fabricated using SD powder, and their complex permeabilities were measured, providing the real part of the initial permeability for SMCs with differing SD powder loadings. Employing identical material parameters, calculations were performed via both the Bruggeman effective medium theory and our proposed algorithm. Figure 5(b) juxtaposes experimental measurements with theoretical predictions for the real part of the initial complex permeability of SD-based SMC. At lower volume fractions, the Bruggeman theory aligns closely with experimental data. However, as the volume fraction increases, the Bruggeman theory deviates significantly from experimental results, while our algorithm maintains consistent alignment with measurements. Notably, due to constraints related to air gaps in the composites, samples with a maximum volume fraction of 60% were produced in this study. It was found that up to a volume fraction of 80%, the impact on the effective permeability of SMCs was relatively limited. Conversely, beyond a volume fraction of 80%, a significant increase in the effective permeability of SMCs could be achieved by increasing the volume fraction. Hence, optimizing the performance of SMCs in future studies may involve increasing their volume fraction.

    Figure 6 presents a comparison between the experimental and calculated complex permeability for 50 vol% Y2Co17/PU composites fabricated with different particle sizes: (a) BD powder and (b) SD powder. In both panels, the red solid lines signify predictions from our algorithm, while blue dashed lines represent uncorrected predictions that overlook skin effect considerations. As the particle size of the metallic magnetic particles increases, several changes occur: the peak position of the imaginary permeability shifts to lower frequencies, peak broadening occurs, and the cut-off frequency decreases.

    Examining the results in Fig. 6(a), significant discrepancies arise between uncorrected calculations and experimental data when skin effects are neglected. In contrast, our algorithm accurately predicts experimental results, underscoring the importance of skin effect corrections for large particle sizes and affirming the efficacy of our approach.

    Notably, discrepancies exist between predicted complex permeability from our algorithm and experimental values for BD powder composite samples (as depicted in Fig. 6(a)). This deviation is attributed to the single-domain particle assumption adopted in our model. For large-sized magnetic particles, the presence of internal domain walls increases, rendering the single-domain assumption invalid and causing discrepancies between calculated results and experimental data. This phenomenon highlights the necessity of fully considering internal magnetic domain structures when calculating the permeability of large particles.

5.   Conclusion
  • This study introduces a novel algorithm devised to calculate the effective permeability of easy-plane metallic SMC. The intrinsic permeability of particle ensembles was determined using the LLG equation tailored for easy-plane systems, combined with a model for magnetic moment orientation distribution. Subsequently, the HEMT was employed to estimate the effective permeability of the composites. Furthermore, skin effect corrections were incorporated to address the impact of particle size on permeability. Experimental results demonstrate the efficacy of the proposed algorithm in accurately predicting the complex permeability of easy-plane metallic SMC with diverse volume fractions and particle sizes. Based on the experimental findings, future efforts to enhance SMC performance should focus on adjusting the volume fraction, controlling particle size, and regulating anisotropy fields. This study effectively bridges the microscale characteristics of easy-plane metallic SMC (intrinsic particle parameters and distribution states) with their macroscale high-frequency magnetic properties (effective permeability), providing a critical theoretical foundation for the design and optimization of soft magnetic materials in the high-frequency range.

Figure (6)  Reference (40)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return