HTML
-
Single-walled carbon nanotubes (SWCNTs) are a unique class of carbon-based materials that possess remarkable properties, including strong carbon–carbon bonds, a non-suspended bonding structure, an ultra-small diameter, and high carrier mobility.[1] These distinctive characteristics make SWCNT-based electronic devices one of the most promising candidates for next-generation nanoelectronics,[2–5] with broad potential applications in fields such as space exploration and nuclear energy industries. However, the operational environments of these devices invariably expose them to various types of radiation. Therefore, investigating the radiation effects on SWCNT-based devices is of great significance and has recently garnered increasing attention.[6–8]
Radiation effects generally include ionizing damage and displacement damage (DD).[9] Recent research has extensively focused on the ionizing damage effects on SWCNT devices, including gamma-ray-induced total ionizing dose (TID) effects,[10–14] as well as single-event effects caused by energetic particle irradiation.[15–17] With regard to DD effects, they refer to the displacement of atomic nuclei caused by interactions with high-energy particles, leading to disruptions in the atomic lattice structure and consequential alterations in material properties. To date, only a limited number of studies have explored the DD effects of SWCNT materials and devices.[18–20] Notably, Peng et al.[5] conducted an evaluation of the DD effects on high-purity semiconductor-type SWCNT transistors using high-energy xenon ions (Xe+) with an energy of 2225 MeV and an ion fluence of 5 × 1012 ions/cm2. Their results revealed that SWCNT transistors exhibited remarkable resistance to radiation compared with silicon transistors in high-energy radiation environments.[21] However, radiation environments vary significantly in terms of particle types and energy levels. Galactic cosmic rays and solar energetic particles can reach energies up to hundreds of MeV or even GeV. Nevertheless, low-energy ion irradiation, such as that encountered in ion implantation processes and scientific instruments, may involve heavy ions with energies ranging from keV to hundreds of keV.[22–25] While the previous study[21] revealed the DD mechanisms in SWCNT devices under high-energy irradiation (2225 MeV Xe+), it was found that SWCNT devices exhibit favourable tolerance to high-energy heavy-ion irradiation. The effects of low-energy ions remain insufficiently explored, and the effects they induce may vary considerably depending on the ion energies.
Therefore, in this paper, we examine the radiation effects induced by low-energy (5 keV) gallium ions (Ga+) on single-walled carbon nanotube field-effect transistors (SWCNT FETs). We analyze the Raman and electrical properties of irradiated SWCNT FETs. The results reveal that SWCNT FETs exhibit lower tolerance to low-energy Ga+ irradiation, resulting in more significant DD compared with higher-energy irradiation. These findings offer valuable insights into the radiation resistance of SWCNT devices and contribute to a better understanding of their performance in various radiation environments.
-
SWCNT FETs were fabricated using semiconductor processes. Figure 1(a) shows the structure of the SWCNT FETs investigated in this study, featuring a back-gate configuration with a SWCNT network film as the conductive channel. The transistors were prepared on a 50 nanometre (nm) SiO2 layer with a heavily P-doped silicon substrate serving as the back gate. The channel dimensions were 60 μm in width and 10 μm in length. The preparation process involved deep reactive ion etching (DRIE) of the silicon wafer using oxygen plasma to increase its hydrophilicity. The wafer was then immersed in a 0.1% aqueous solution of poly-L-lysine (PLL) to enable functionalization with a semiconducting SWCNT solution. Figure 1(b) displays the scanning electron microscope (SEM) image of the prepared SWCNT film, exhibiting a uniformly distributed array with good quality. The SWCNT thin film was patterned using photolithography, followed by the deposition of Ti and Au to form the source and drain contacts. Oxygen plasma etching was then used to selectively remove SWCNTs between the contacts, achieving precise channel dimensions and electrical isolation.
In this work, Ga+ irradiation experiments were conducted using the Thermo Scientific Helios FIB–SEM DualBeam system. The irradiation experiments were carried out at an acceleration voltage of 5 keV and a beam current of 3 pA. To ensure reliable results, ten SWCNT FETs with uniform dimensions and electrical characteristics were carefully selected, as shown in Fig. 1(c). These transistors exhibited consistent and predictable electrical behavior, with well-defined current–voltage (I–V) characteristics and consistent threshold voltage values before irradiation. This consistency provided a baseline for comparing changes or degradation in performance due to Ga+ irradiation. The uniformity in both dimensions and electrical properties among the selected SWCNT FETs ensured that any observed changes in their performance after irradiation could be attributed to radiation effects rather than inconsistencies in fabrication or initial conditions. Subsequently, irradiation experiments were carried out on these SWCNT FETs with varying fluences of Ga+ ions. The entire channel area of the SWCNT FETs was exposed to irradiation, as shown in Fig. 1(d). The specific irradiation fluences used in the experiments were as follows: 1 × 1011 ions/cm2, 1 × 1012 ions/cm2, 1 × 1013 ions/cm2, 5 × 1013 ions/cm2, 1 × 1014 ions/cm2, 2.5 × 1014 ions/cm2, 5 × 1014 ions/cm2, 1 × 1015 ions/cm2, and 1 × 1016 ions/cm2. After irradiation, the electrical characteristics of all ten SWCNT FETs exhibited similar trends, and one of them was selected as a representative device for further analysis.
-
Figure 2(a) displays the Raman spectra of the SWCNT channel under different ion fluences. Two key peaks, the D peak at 1350 cm−1 and the G peak at 1580 cm−1, are crucial for analyzing the structural characteristics of the SWCNTs. The D peak indicates the presence of structural defects in SWCNTs, as it corresponds to changes in the stretching vibration mode of carbon–carbon bonds. The G peak, originating from the tangential motion of carbon atoms, reveals the structural integrity of sp2-hybridized carbon, which not only partially reflects the defects of SWCNTs but also distinguishes the conductive types (metallic and semiconducting) of SWCNTs. Figure 2(b) depicts the ratio of the D and G peak intensities (ID/IG+), which is employed to assess the relationship between the intensities of the two peaks. This ratio provides insight into the density of structural defects in SWCNTs. A higher value of ID/IG+ signifies a greater presence of defects, which is utilized to characterize the structural integrity and quality of CNTs.[26] Furthermore, Fig. 2(c) demonstrates the shift in the position of the 2D peak resulting from Ga+ ion irradiation. The 2D peak, also known as the G’ peak, arises from double-phonon scattering in the absence of defect activation. It is a significant parameter for characterizing the degree of SWCNT doping.[27] Shifts in the position of the 2D band can provide insights into changes in the electronic structure and doping effects induced by Ga+ irradiation.
As illustrated in Figs. 2(a) and 2(b), the variation trends of ID/IG+ from Raman spectra, along with the corresponding changes in electrical properties, exhibit three distinct phases of alteration. Phase I: for Ga+ ion fluences ranging from 1 × 1011 ions/cm2 to 1 × 1014 ions/cm2, the D peak intensity shows a slight enhancement when Ga+ ions irradiate the pristine SWCNT at a fluence of 1 × 1011 ions/cm2. Minimal changes are observed in the Raman spectra until the fluence reaches 1 × 1014 ions/cm2, where noticeable broadening of the D and G peaks occurs. Phase II: with Ga+ ion fluences ranging from 2.5 × 1014 ions/cm2 to 5 × 1014 ions/cm2, the peak broadening continues, and the 2D peak becomes nearly invisible, indicating a significant alteration in the nanotube structure. Phase III: for Ga+ ion fluences ranging from 1 × 1015 ions/cm2 to 1 × 1016 ions/cm2, the D and G peaks lose their distinct shapes, reflecting substantial structural degradation of the SWCNTs.
Figure 2(b) shows that the Raman spectrum of pristine SWCNT exhibits a very small ID/IG+ ratio, indicating minimal defects prior to irradiation. In phase I, there is a significant increase in ID/IG+ compared with the initial value when the Ga+ fluence is 1 × 1011 ions/cm2, indicating that Ga+ irradiation causes substantial DD to the lattice. The ID/IG+ remains relatively stable for fluences ranging from 1 × 1011 ions/cm2 to 1 × 1013 ions/cm2, with no significant change in surface defect concentration. At a Ga+ fluence of 1 × 1014 ions/cm2, the ID/IG+ reaches its maximum value, reflecting the peak defect concentration within the SWCNT and confirming that a fluence of 1 × 1014 ions/cm2 with 5 keV Ga+ irradiation causes significant DD to the SWCNT. In phase II, as the Ga+ fluence exceeds 1 × 1014 ions/cm2, the SWCNT begins to undergo amorphization, and at fluences beyond 5 × 1014 ions/cm2, the ID/IG+ no longer serves as a reliable indicator, suggesting that the SWCNTs have experienced significant amorphization.
It is evident from Fig. 2(c) that prior to the disappearance of the 2D peak of the SWCNT, a shift towards a lower wavenumber is observed. This shift becomes more pronounced as the Ga+ irradiation fluence increases. This shift suggests that the electron concentration within the SWCNT increases after irradiation. This phenomenon can be explained by the fact that 5 keV Ga+ ions are predominantly located in the SWCNT film channels or within the SiO2 layer located only a few nm away from the channels. Since the transistor itself is not annealed, Ga+ ions can retain bound charges, which induce charge transfer and generate electrons in the channel, leading to the observed redshift of the 2D peak.
-
Furthermore, the electrical properties of SWCNT FETs were analyzed both before and after irradiation to obtain a deeper understanding of the relationship between DD and the observed changes in SWCNT FETs. Notably, the variations in the electrical properties followed the same three-phase trend as the Raman spectra.
In Fig. 3(a), the transfer characteristic curves of SWCNT FETs before and after irradiation with different Ga+ ion fluences are demonstrated, where the grey curves represent the pristine transfer characteristics of the devices. Figure 3(b) illustrates the trends of the on-state current (Ion), off-state current (Ioff), and gate leakage current of the SWCNT FETs across the three fluence phases. Figure 3(c) displays the corresponding variations in the subthreshold swing (SS) and Ion/Ioff ratio. It is evident that in Phase I, the electrical properties of SWCNT FETs show a significant decrease, especially after irradiation with a Ga+ fluence of 1 × 1011 ions/cm2, where the most significant degradation in electrical performance is observed. This degradation is attributed to the generation of vacancy defects in the SWCNTs by Ga+ irradiation, which disrupts the channel conductivity.
In phase I, when the Ga+ fluence is 1 × 1011 ions/cm2, the performance of SWCNT FETs shows substantial degradation, as shown in Figs. 3(b) and 3(c). Notably, the Ion decreases by one order of magnitude, and the Ion/Ioff ratio decreases by two orders of magnitude. Simultaneously, the Ioff, gate leakage current, and SS all increase. This degradation is likely due to the generation of vacancy defects in the SWCNT film channel and gate oxide layer, which increase the gate leakage current and thereby affect the gate modulation efficiency. Despite the increased gate leakage current, the gate retains a certain modulation capability, as indicated by the transfer characteristics and gate leakage current magnitude. Instead, the increased gate leakage current is attributed to trap-assisted tunneling (TAT), where electrons tunnel through trap states associated with vacancy defects in the gate oxide layer under the applied gate bias.[28,29] While TAT increases the gate leakage current (affecting Ioff) and does not significantly impact Ion, it does not completely destroy the transistor’s functionality. Notably, the magnitude of this TAT-induced leakage increase appears to be fluence independent in this phase. At an ion fluence of 1 × 1014 ions/cm2, the SS is restored to the pre-irradiation level, and the Ion/Ioff ratio exceeds 103. The gate leakage current, however, does not continue to increase. This suggests that the degree of damage to the gate oxide caused by Ga+ ions does not show a positive correlation with ion fluence. This phenomenon is likely attributed to the presence of surface contamination, such as air doping and impurities remaining from the fabrication process, as well as the formation of interface states at the gate oxide/SWCNT interface.
In phase II, as shown in Fig. 3(b), when the Ga+ fluence exceeds 1 × 1014 ions/cm2, the Ion remains almost unchanged, and ID/IG+ reaches its maximum. This suggests that a large number of defects have formed in the SWCNTs and have reached saturation. In this case, the current cannot be redistributed between the damaged and undamaged SWCNTs, suggesting defect saturation within the SWCNT network. At this point, further damage does not significantly alter the overall conductive pathways or the Ion. The continued increase in gate leakage current with fluence directly contributes to the rise in Ioff and SS. This can be attributed to the increased electron concentration in the SWCNTs. The variation of the 2D peak shift of the SWCNT channel with irradiation fluence further supports this explanation, as shown in Fig. 2(c). A redshift in the peak position becomes more pronounced with increasing Ga+ ion fluence, indicating an increase in the electron concentration within the irradiated SWCNTs. This phenomenon can be explained by the fact that 5 keV Ga+ ions primarily reside in the SWCNT film channel or within the SiO2 layer located a few nanometers from the channel after irradiation. Since the FETs were not annealed, Ga+ ions may retain bound charges, inducing additional charge and resulting in the generation of extra electrons in the channel. These extra electrons contribute to the increased SS and Ioff of the transistor.
In phase III, the transistor exhibits a significant decline in both Ion and Ioff. This reduction can be ascribed to the elevated fluence levels of Ga+ ion irradiation causing severe DD in the SWCNT film channel, leading to complete amorphization of the film. Consequently, the structural integrity of the SWCNTs is severely compromised, leading to the loss of their conductive properties.
The experimental results reveal that SWCNT FETs exhibit limited tolerance to low-energy Ga+ ion irradiation, in contrast to their high tolerance when exposed to high-energy heavy-ion (2225 MeV Xe+) irradiation.[21] While the device structure plays an important role, the primary factor lies in the ion parameters. When the SWCNTs were irradiated by 2225 MeV Xe+ with a fluence of 1 × 1012 ions/cm2, minimal damage occurred to both the SWCNT channel and the gate oxide layer, as indicated by negligible changes in ID/IG+ and the gate leakage current. Conversely, significant changes were observed in both the current-carrying capacity of the channel and the insulation properties of the SWCNT FETs under low-energy Ga+ irradiation. We attribute this discrepancy to the much higher DD caused by low-energy heavy ions compared with high-energy heavy ions. Low- energy Ga+ ions cause localized damage with a higher energy density, resulting in more substantial atomic displacement and defect generation within the SWCNTs and the gate oxide layer, which severely degrades the device performance, including decreases in Ion and Ion/Ioff, reflecting the diminished current-carrying capability of the devices. Such degradation leads to gain reduction, increased power consumption, and impaired noise performance in analog circuits. A rise in SS and gate leakage current indicates deteriorated switching behavior. In digital logic circuits, these impairments result in reduced operating speed, higher static power dissipation, and potential functional failures in integrated systems. In comparison, high-energy Xe+ ions penetrate deeper and distribute their energy over a larger volume, causing less localized damage and consequently having minimal effects on the SWCNTs and gate oxide layer.
-
To quantitatively compare the severity of DD induced by low-energy and high-energy heavy ions, TRIM[30] software based on the Monte Carlo method was used to simulate the radiation effects of heavy ions across a broad energy range. In the simulation, Ga+ and Xe+ with energies ranging from 5 keV to 2200 MeV were selected as radiation sources, with a uniform total fluence of 1 × 1012 ions/cm2. Due to the absence of a direct SWCNT model in TRIM, the SWCNT was approximated using a graphite-graphite (ultra-low density)-graphite model, with thicknesses of 0.5 nm, 1 nm, and 0.5 nm, respectively, on a 50 nm SiO2 substrate, as shown in Fig. 4(a). By employing Monte Carlo simulations, we are able to analyze the damage caused by ions of varying energies and assess the impact of the SWCNT film thickness and substrate material on the overall behavior of SWCNT FETs.
Here, we focused on the DD caused by primary knock-on atoms (PKAs) and the energy loss of charged particles in the material to provide a quantitative description of the influence of heavy-ion irradiation on SWCNT FETs. When particles with sufficient energy interact with lattice atoms, they transfer energy to displace atoms from their original positions. These displaced atoms are known as PKAs.[31] PKAs are typically in an ionized state, and if they possess sufficient energy, they can induce additional DD by colliding with other lattice atoms, causing further displacements.[32] Figures 4(b) and 4(d) show that at an energy of 5 keV, the PKAs and point defects generated by Ga+ and Xe+ are mainly distributed in the SWCNT film and at the interface between the gate oxide layer and the SWCNT. However, at higher ion energies of 50 keV, Ga+ and Xe+ ions have sufficient energy to penetrate the gate oxide layer and produce PKAs as well as vacancies within it, leading to an increase in vacancy defects in the gate oxide layer. As the ion energy continues to increase, the total number of vacancies in SWCNT FETs decreases. At the highest ion energy of 2200 MeV for both ions, the curve representing the number of vacancies exhibits minimal variation, suggesting that the generation of PKA-induced defects in both the SWCNTs and gate oxide layers is significantly suppressed compared with low-energy ion irradiation. This is because high-energy ions penetrate both the SWCNT and gate oxide layers, reducing continuous defect generation. It is noteworthy that, although Xe+ produces more vacancies than Ga+ at an energy of 500 keV, this difference is attributed to the atomic mass and volume. However, in terms of the variation trends of energy and vacancies, Ga+ and Xe+ ions show similar patterns. Therefore, the results indicate that ion energy is the dominant factor affecting PKA generation and vacancy defects.
As demonstrated by the simulation results, the generation of PKAs and defects in SWCNT FETs is significantly impacted by the energy of ion irradiation. These results are further analyzed in terms of energy deposition obtained from the simulations. When ions interact with materials, they induce two types of damage: ionization energy loss (IEL) and non-ionization energy loss (NIEL).[33] IEL refers to energy deposited via electronic excitation and ionization, creating electron-hole pairs. NIEL refers to energy deposited via elastic nuclear collisions, leading to atomic displacements (creating PKAs and vacancies) and phonon generation. Atomic displacement is primarily caused by elastic nuclear collisions (Coulomb scattering with nuclei). Figures 4(c) and 4(e) illustrate the variations in the number of PKAs, elemental vacancies, and energy deposition from both ionization and non-ionization processes as a function of incident ion energy, with an ion fluence of 1 × 1012 ions/cm2. The results reveal that the highest number of vacancies occurs at an energy of 50 keV for both Ga+ and Xe+. However, both the number of PKAs and vacancies decrease with increasing ion energy, with the number of vacancies dropping significantly for energies above 500 MeV. At lower ion energies, NIEL dominates the energy deposition process, with phonons and atomic displacements being the primary forms of damage. In contrast, as the ion energy increases, the cross-section for ionizing collisions increases, leading to a higher probability of ionization. This results in less energy deposition through non-ionization processes. At very high ion energies (e.g., 2225 MeV), ionization energy deposition surpasses non-ionization energy deposition almost entirely. As a result, both the SWCNT film and the gate oxide layer show very few vacancies. In addition, the displacement damage dose (Dd) provides a unified quantitative standard for assessing the degree of damage to materials under different irradiation fluences. It can be calculated using[21,34]
As shown in Figs. 4(c) and 4(e), the Dd values for Xe+ at 5 keV and 2200 MeV are 1.25 × 1015 MeV/g and 1.5 × 1013 MeV/g, respectively, which are consistent with the values reported in Ref. [21] (2.79 × 1013 MeV/g for 2225 MeV Xe+), while the Dd values for Ga+ at 5 keV and 2200 MeV are 1.19 × 1015 MeV/g and 3.4 × 1012 MeV/g, respectively. It can be seen that the Dd produced by 5 keV Ga+ is nearly three orders of magnitude higher than that produced by high-energy ions (2225 MeV Xe+). The simulation results align with the experimental findings, indicating that the vacancy defects induced by 5 keV Ga+ ions are mainly localized in the SWCNT material and gate oxide layer.
3.1. Raman analysis
3.2. Electrical characterization
3.3. TRIM simulation and damage mechanism
-
In conclusion, the effects of low-energy Ga+ irradiation on SWCNT FETs were systematically investigated. Raman spectroscopy and electrical measurements revealed that low-energy Ga+ irradiation (5 keV) induces severe DD in SWCNTs, significantly degrading the current-carrying capacity of the channel and compromising the insulating properties of the gate oxide. As a result, the electrical properties of SWCNT FETs degrade, suggesting heightened vulnerability to low-energy heavy-ion irradiation. The simulation results further validate these observations, showing that low-energy ions generate significantly more atomic displacements and vacancies (DD) compared with high-energy ions. This is because low-energy ions primarily deposit energy through non-ionization mechanisms, which lead to atomic displacements and defect generation. In contrast, high-energy ions deposit energy mainly through ionization, leading to fewer atomic displacements and defects, and ultimately less damage to SWCNTs and SWCNT FETs. This research underscores the importance of considering ion energy when designing and evaluating SWCNT-based devices, especially for applications in environments with high radiation exposure. The findings suggest that SWCNT FETs, while promising for a range of applications, may require further development to enhance their tolerance to radiation-induced damage, particularly in low-energy ion environments.