Heat can be converted to electricity directly using thermoelectric materials, which are valuable in waste heat power generation, outdoor portable power supply, etc., and have garnered tremendous research attention due to the current energy and environmental issues.[1–3] The thermoelectric conversion efficiency of a material is described by a dimensionless quality factor, called figure of merit (ZT) with ZT = S2σT/ (Ke + Kph). Here, S is the Seebeck coefficient, σ is electrical conductance, Ke is electronic thermal conductance, Kph is phonon thermal conductance, and T is absolute temperature. So to realize high thermoelectric conversion efficiency, the thermoelectric material should have a large Seebeck coefficient S and electronic conductance σ, and a low electrical and phonon thermal conductance (Ke and Kph). However, a high electronic conductance σ is usually accompanied by a high electronic thermal conductance Ke via the Wiedemann–Franz law, and a high Seebeck coefficient S is often accompanied by lower electrical conductance σ.[4,5] So optimizing these transport coefficients simultaneously is tough because they are strongly coupled with each other and cannot independently enhance the thermoelectric performance of a material.[6–8] Fortunately, it has been reported that the Wiedemann–Franz law is not as applicable in nanoscale systems as in bulk materials.[9,10] Consequently, research efforts have increasingly focused on the thermoelectric properties of two-dimensional (2D) materials. In atomically thin monolayers, the power factors can be enhanced by strategic band structure engineering[11–14] and the carrier mobility can be significantly improved via reducing effective mass based on the quantum confinement effect; meanwhile, the phonon scattering can be improved because of the multiscale distribution of interlayer interfaces, grain boundaries, and defects in two-dimensional monolayer materials.[15,16] For instance, Pathak et al. demonstrated a high ZT of 1.55 at 865 K in doped SnTe, where a co-doping strategy of Ag and Mg in self-compensated Sn1.03Te effectively reduces the thermal conductance and improves the power factor,[17] and Liu et al. reported that in the layered structure of SnSe, point defects are critical tools for precisely regulating carrier concentration and band structure, with the power factor (S2σ) increasing from ∼8 μW ⋅ cm−1 ⋅ K−2 to ∼ 31.5 μW ⋅ cm−1 ⋅ K−2 at 623 K.[18] Jia et al. systematically investigated the thermoelectric properties of MoS2/MoSe2 van der Waals heterostructures and found that the van der Waals heterostructure induces strong localization of electrons and phonons due to interface effects, significantly reducing thermal conductance, with the phonon thermal conductance Kph reduced to ∼5 pW/K at 300 K.[19] Jue Wang et al. proposed that monolayer MoS2–MoSe2 aperiodic superlattices can effectively reduce phonon thermal conductance and reach a ZT of 1.38 at 500 K.[20] Stimulated by the in-plane lateral heterostructure in the application of thermoelectric devices, Song and Sun demonstrated that twist angle engineering in WSe2/MoSe2 superlattice heterostructures optimizes the carrier concentration and band gap, achieving a peak ZT of 1.35 at 600 K and a twist angle of 21.79° due to enhanced power factor and reduced thermal conductance.[21]
Janus transition metal dichalcogenides (TMDs), a distinctive class of two-dimensional (2D) materials characterized by out-of-plane structural symmetry breaking arising from the composition of each layer with distinct elements differing in atomic radius, electronegativity, and atomic mass, demonstrate a favorable combination of relatively high electrical transport efficiency and low Kph, which exhibits significant promise for thermoelectric applications.[22–28] Zhang et al. demonstrated that Janus materials with their atomic mass differences can greatly optimize phonon scattering,[22] and Patel et al. demonstrated that the Janus WSTe monolayer exhibits ultralow Kph, which is nearly 150 times smaller than WS2 and 100 times smaller than WSSe near room temperature due to out-of-plane structural asymmetry disrupting phonon dispersion, and concurrently, its Seebeck coefficient S reaches 322 μV/K owing to asymmetric band structures, yielding a high ZT of 2.56 at 1200 K.[23] Xiong et al. further introduced disorder through atomic positional tuning and achieved significant thermoelectric improvements in Janus MoSSe. They found the atomic disorder in Janus MoSSe induces local atomic-level resonance, increases the electronic density of states and improves S, and simultaneously decreases Kph.[25] So local structural tuning at the atomic scale is an effective means to obtain high thermoelectric performance.
Compared to the Janus MoSSe monolayer and WSTe monolayer,[24,26] the Janus MoTeS monolayer shows a more significant difference in atomic radius and mass between the Te and S layers, which may result in stronger phonon scattering. Here, we further study this atomic-scale tuning method of the effect of periodic alternation of intrinsic elements on electronic and phonon transport, aiming to realize high thermoelectric performance in MoTeS constructed devices. In the work, first-principles are implemented to explore the thermoelectric performance of Janus MoTeS, mainly focusing on the high-frequency (S/Te) alternations and van der Waals heterojunctions to enhance ZT. It is shown that increasing the alternation frequency in the transport direction can enhance the Seebeck coefficient S and simultaneously suppress the phonon thermal conductance Kph, yielding ZT of 1.58 at 300 K in the high-frequency alternating (HFA) structure. Further, the phonon thermal conductance Kph decreases greatly when the HFA monolayer device is extended into a van der Waals heterojunction, resulting in a high ZT of 1.80 at 300 K, which rises to 3.49 at 500 K. This work is useful in designing high-performance thermoelectric materials via periodic structural alternations.
-
The thermoelectric transport properties are calculated using density functional theory (DFT) combined with the non-equilibrium Green’s function (NEGF) method, and calculations are performed with the Atomistix ToolKit package.[29,30] The generalized gradient approximation (GGA) and Perdew–Burke–Ernzerhof (PBE) are used to describe the exchange–correlation potential of electrons.[31] Before calculations of the transport properties, all device structures are fully optimized, with a convergence criterion for structural relaxation set at a force on each atom less than 0.02 eV⋅Å−1. The double-zeta polarized (DZP) basis set is employed to describe the localized atomic orbitals.[32,33] The cut-off energy for the real-space grid is set at 85 Hartree. The convergence criterion for the total energy is set to 10−5 Hartree. The electronic temperature is set at 300 K. Periodic boundary conditions are applied in the x direction to eliminate the influence of edges, and a vacuum layer with a thickness of 15 Å is used in the y direction to avoid interactions. The DFT-D2 empirical correction approach is utilized to accurately model the physical attributes of layered materials characterized by weak van der Waals (vdW) interactions.[34]
The electronic transmission spectrum Te (ε) is calculated by using the NEGF method. Based on the Caroli formula, the electronic transmission can be given as[35]
Then, the electronic conductance (σ), Seebeck coefficient (S), and electronic thermal conductance (Ke) as functions of the chemical potential can be expressed as follows:[36,37]
The Lorenz function can be represented as
where f(E, μ, T) is the Fermi–Dirac distribution (a function of E, temperature T and chemical potential μ). The phonon transmission function Tph(ω) is given by a Caroli type formula, where ω is the phonon frequency. The phonon transmission function is
In this case, the phononic contribution to thermal conductance (Kph) is calculated using the methodology outlined in Ref. [38] with the governing equation[39]
where fBE(ω, T) is the Bose–Einstein distribution function, T is the average temperature of the whole device and ω stands for the phonon frequency. The electronic thermal conductance Ke is calculated directly from the electron transmission spectrum using Eq. (4).
-
In order to study the effect of periodic alternation of the intrinsic elements S and Te on the thermoelectric performance, three configurations are constructed based on the two-dimensional material MoTeS, including the low-frequency alternating (LFA) structure, the high-frequency alternating (HFA) structure, and the pristine monolayer structure for comparison, as shown in Fig. 1. Each device consists of three regions: the left and right electrodes and a central scattering region. The pristine Janus structure, as shown in Fig. 1(a), features sulfur (S) and tellurium (Te) atoms positioned on opposing top and bottom surfaces. The LFA structure, depicted in Fig. 1(b), exhibits a periodic alternation of S and Te atoms along the transport direction with a period of two unit cells; as highlighted in the blue box, within one period, half of the adjacent S atoms on the top surface are substituted with Te atoms, and S atoms occupy corresponding positions on the bottom surface. The HFA structure, shown in Fig. 1(c), has a period of one unit cell, with a surface atomic arrangement similar to the LFA but higher-frequency alternation than the LFA.
The temperature dependence of phonon thermal conductance Kph for the three configurations is illustrated in Fig. 2(a). The Kph for all three configurations rises rapidly as the temperature increases at the beginning and then nearly stabilizes when the temperature is beyond 300 K. However, a significantly lower Kph is observed in the LFA structure as compared to pristine MoTeS, attributed to the periodic structural alternation. This reduction in Kph is further enhanced in the HFA structure, resulting from further enhanced phonon-interface scattering. Specifically, the phonon thermal conductance Kph for the HFA structure is reduced to 67% of that for the pristine MoTeS structure. According to the formula of the phonon thermal conductance,[39] the total phonon transmission Tph makes a great contribution to the phonon thermal conductance. It can be seen from Fig. 2(b) that marked suppression of phonon transmission is observed in the LFA and HFA structures relative to the pristine structure, nearly over all phonon frequencies except near 35 meV and 20 meV. The transmission coefficients for the HFA structure at low-frequency phonons near the energy 12 meV and the energy ranges 22–32 meV decrease much more significantly as compared to those for the LFA structure, which results in the lowest phonon thermal conductance Kph in the HFA structure.
To demonstrate the specific contributions of different phonon modes to phonon transmission, the calculated local phonon density of states (LPDOS) for them is presented in Fig. 3. The phonon density of states of the pristine structure has values over the whole range of phonon frequencies except near 35 meV and 20 meV as shown in Fig. 3(b), which means that phonons in the left electrode can transmit through the central region and reach the right electrode easily, leading to the high phonon transmission as shown in Fig. 2(b). Moreover, its large values are mainly concentrated in the energy ranges 10–18 meV and 22–32 meV, which induces higher Kph due to the dominance of low-frequency phonons in heat transfer.[40] As shown in Fig. 3(b), LFA exhibits a reduction in LPDOS within the 22–32 meV range. This suppression is directly attributed to periodic defects, which simultaneously block phonon propagation at these specific energies and enhance phonon scattering.[41,42] This effect is further amplified in HFA as shown in Fig. 3(c), which exhibits significantly stronger suppression of the phonon density of states within the 22–32 meV range than that in LFA, resulting in substantially reduced Tph and Kph. Notably, as the frequency of periodic alternation defects increases, phonon transport becomes progressively impeded.
The distribution of local phonon density of states (LPDOS) projected along the z-direction is presented for (a) pristine MoTeS, (b) LFA, and (c) HFA configurations. The color scale indicates the magnitude of the LPDOS at each spatial point and frequency.
Subsequently, the electronic transport and thermoelectric performance of pristine MoTeS, LFA, and HFA structures are investigated. As shown in Fig. 4(a), at most electron energies, the electron transmission for the pristine structure has the highest values among the three configurations. This superior transmission originates from its uniform Janus configuration, where sulfur (S) and tellurium (Te) atoms arrange on opposing surfaces, minimizing electron scattering. However, at electron energies from about −1 eV to −0.73 eV, the electron transmission for HFA is greatly enhanced, much higher than that for the pristine structure, which leads to improved electrical conductance as shown in Fig. 4(b). Figure 4(c) displays the Seebeck coefficient as a function of chemical potential. HFA exhibits higher S values than LFA, and pristine MoTeS exhibits μ values in the range from about −0.8 eV to −0.2 eV due to its highly alternating structure. Then the power factor PF = S2σ, a key metric for device thermoelectric performance, reaches its maximum value of 2.46 pW/K2 at μ = −0.73 eV for HFA in Fig. 4(d). The total thermal conductance, comprising electronic and phononic contributions, is presented in Fig. 4(e). The trend in Ke mirrors electrical conductance as shown in Fig. 4(b), confirming their positive correlation. Critically, HFA demonstrates consistently lower Ktotal near μ = −0.73 eV compared to LFA and pristine MoTeS, primarily due to the reduced Kph. Finally, a maximum ZT value of 1.58 for the HFA structure is achieved, much larger than that for the pristine structure (0.43) and LFA (0.77), as shown in Fig. 4(f). This superior ZT in HFA stems from the significant increase in PF and simultaneous suppression of Kph.
-
In order to further improve the thermoelectric properties of Janus MoTeS devices via suppressing Kph deeply, the vdW-HFA heterojunction is constructed with two HFA monolayers stacked via a weak van der Waals junction, as shown in Fig. 1(d). The interlayer contact contains three unit cells, and the interlayer spacing is 3.63 Å in the vdW-HFA heterojunction. The temperature-dependent Kph and corresponding transmission spectra Tph(ω) are presented in Fig. 5. Attributed to enhanced interface scattering, the phonon transmission below 50 meV for vdW-HFA is more deeply suppressed than that for HFA, as shown in Fig. 5(b), accompanied by a substantially lower Kph for vdW-HFA compared with that for HFA, as observed in Fig. 5(a).
The electronic transport and thermoelectric properties for the vdW-HFA structure are shown in Fig. 6 (also presented is that for HFA for comparison). Compared with that for HFA, the electron transmission coefficient for vdW-HFA is also greatly reduced (see Fig. 6(a)) because the weak interlayer coupling in the vdW structure constrains the available transmission channels and hampers the electron tunneling during interlayer propagation (the corresponding analysis will be given later). As a result, the electrical conductance of vdW-HFA is also diminished compared with that of HFA, as can be seen from Fig. 6(b). The S for vdW-HFA is marginally higher than that for HFA, as shown in Fig. 6(c), which is inversely correlated with its reduced electrical conductance (see Fig. 6(c)). The maximum power factors PF for HFA and vdW-HFA occur at the chemical potentials μ of −0.68 eV and 0.81 eV, respectively, with the maximum PF for HFA being approximately twice that of vdW-HFA, as illustrated in Fig. 6(d). This disparity stems from the electrical conductance for vdW-HFA being much lower than that for HFA. The total thermal conductance Ktot of vdW-HFA is substantially lower than that of HFA, as shown in Fig. 6(e), due to the reductions in both Ke and Kph. Although the electron conductance in vdW-HFA is also suppressed greatly, a significantly enhanced figure of merit ZT 1.80 at 300 K is obtained for vdW-HFA (higher than the ZTmax 1.58 for HFA) through pronounced suppression of Ktot via weak interlayer coupling, which prevails over the competing effect of S2σ, as demonstrated in Fig. 6(f).
To give the physical reason why the transmission coefficient and conductance for vdW-HFA are more greatly reduced compared with those for HFA, the local device density of states (LDDOS) for both structures is calculated at the corresponding chemical potentials −0.68 eV for HFA and 0.81 eV for vdW-HFA. As can be seen from Fig. 7, the LDDOS for HFA is distributed on the whole device, so electrons can transmit through easily, resulting in the rather high transmission coefficient and conductance, whereas in the vdW-HFA, it remains highly localized and confined, which makes it hard for electrons to traverse the van der Waals interface, leading to the smaller transmission coefficient and conductance. Similar analysis can also be applied to the Ke difference between the HFA and vdW-HFA.
The maximum ZTmax values for both HFA and vdW-HFA increase with the increase of temperature within the considered temperature range from 100 K to 500 K, as shown in Fig. 8. A pronounced temperature-dependent enhancement of the ZTmax value for vdW-HFA is observed, surpassing that for HFA at approximately 200 K. Beyond 200 K, the substantial reduction in Kph for vdW-HFA prevails over the lower PF, resulting in a higher ZT relative to HFA. What is more, the maximum ZTmax value for vdW-HFA rises to 3.49 as the temperature increases to 500 K. Then, how does the temperature increase lead to the enhancement of ZT from 1.80 to 3.49? As can be seen from Table 1, the significant enhancement of ZTmax from 1.80 at 300 K to 3.49 at 500 K is primarily driven by the synergistic effects of temperature on the thermoelectric parameters: the Seebeck coefficient S increases markedly from 0.24 mV/K to 0.31 mV/K, resulting in a substantial 58% improvement in the power factor (S2σ) from 0.79 pW/K2 to 1.25 pW/K2 though the electrical conductivity σ experiences a slight decrease from 13.69 μS to approximately 12.98 μS. In addition, the total thermal conductivity Ktot is nearly stable as the phonon thermal conductivity Kph and the electronic thermal conductivity Ke remain nearly unchanged. The temperature T in the numerator of the ZT expression acts as a linear amplifier, and its increase from 300 K to 500 K (a 67% rise) directly magnifies the gain in (S2σT). The overall growth of the numerator (S2σ) by 163% vastly outweighs the minimal change in the denominator (Ktot), thereby dominating the enhancement of ZT and demonstrating the outstanding high-temperature thermoelectric performance of the vdW-HFA junction.
3.1. Influence of alternation frequency on thermoelectric performance
3.2. Influence of weak coupling interfaces on thermoelectric performance
-
In summary, the thermoelectric performance of Janus MoTeS-based devices were studied by first-principles calculations based on density functional theory. Firstly, we investigated the impact of period S–Te atom alternation frequency on the thermoelectric performance of Janus MoTeS-based devices, as the two-dimensional Janus MoTeS has inherent out-of-plane asymmetry. Among the three configurations with different alternation frequencies, the HFA structure demonstrated superior thermoelectric performance as the Seebeck coefficient was enhanced and the phonon thermal conductance was suppressed simultaneously when the alternation frequency of the structure in the transport direction increased. A maximum ZT of 1.58 was obtained in the HFA structure at 300 K. Then, in order to further improve the thermoelectric properties of Janus MoTeS devices via suppressing Kph deeply, the vdW-HFA heterojunction was constructed with two HFA monolayers stacked via a weak van der Waals junction. Indeed, the phonon thermal conductance decreased greatly, resulting in a high ZT of 1.80 at 300 K, which rose to 3.49 as the temperature increased to 500 K, and in experiments, techniques such as stepwise growth processes have demonstrated the feasibility of creating atomically sharp interfaces within layered materials. The results suggest that atomic-level structural design plays an important role in modulating the thermoelectric properties of Janus 2D materials, which is useful for further exploration of their device applications.