2026 Volume 35 Issue 7
Article Contents

Jing-Jing Xing, Shunran Liu, Ren-Liang Zhang, Yong-Gang Wang, Li-Jun Yi. Minimum grain size and compression mechanical behavior of polycrystalline graphene based carbon honeycombs: Cell irregularity and grain size effect[J]. Chinese Physics B, 2026, 35(7): 076103. doi: 10.1088/1674-1056/ae12d1
Citation: Jing-Jing Xing, Shunran Liu, Ren-Liang Zhang, Yong-Gang Wang, Li-Jun Yi. Minimum grain size and compression mechanical behavior of polycrystalline graphene based carbon honeycombs: Cell irregularity and grain size effect[J]. Chinese Physics B, 2026, 35(7): 076103. doi: 10.1088/1674-1056/ae12d1

Minimum grain size and compression mechanical behavior of polycrystalline graphene based carbon honeycombs: Cell irregularity and grain size effect

  • Received Date: 20/07/2025
    Accepted Date: 05/10/2025
    Available Online: 01/07/2026
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(9)  /  Tables(2)

Article Metrics

Article views(111) PDF downloads(0) Cited by(0)

Access History

Minimum grain size and compression mechanical behavior of polycrystalline graphene based carbon honeycombs: Cell irregularity and grain size effect

Abstract: The graphene-based carbon honeycombs (CHCs) have excellent mechanical properties and various applications, and have attracted intensive attention recently. However, the real CHCs in experiments have random cell shapes. The effects of polycrystallinity and cell irregularity on the mechanical properties of CHCs are still unknown. Here, first, we investigate the minimum cell size stability with ideal cell walls in the polycrystalline graphene-based carbon honeycombs (PGCHs). Then, based on molecular dynamics simulations, the compressive mechanical properties of four PGCHs with typical cell irregularities are studied systematically, including the periodic regular graphene-based carbon honeycombs (RGCHs) with a zero-degree cell irregularity. Under in-plane compression, the Young’s modulus, initial peak stress, mean plateau stress, and per volume energy absorption Wv of RGCHs and PGCHs decrease significantly with increasing grain size, and show a pseudo Hall–Petch relation. The mean plateau stress and Wv of PGCHs are higher than those of RGCHs. Under out-of-plane compression, the grain size effect is also obvious. However, the influence of cell irregularity is very small and can be ignored. The results indicate that the Hall–Petch relations of polycrystalline materials are dependent on both grain size and cell irregularity, and provide theoretical guidance for real CHCs in engineering applications.

1.   Introduction
  • Carbon honeycomb is a three-dimensional (3D) cellular structure consisting of graphene nanoribbons,[1] and attracts wide attention due to unique physical and chemical properties. Carbon honeycomb shows distinctive electronic and magnetic properties,[2–4] excellent mechanical properties,[5–9] high thermal conductivity.[8–11] It has excellent potential applications, such as high adsorption and storage capacity for gaseous and liquid species,[1,2,12] and excellent anti-impact energy absorption.[6,7,13] Carbon honeycomb may also possess potential applications in nanoscale resonators and heat transfer.[14–16] However, although the real carbon honeycomb is always in a polycrystalline structure state in experiment,[1,17] most previous studies are based on periodic regular graphene-based carbon honeycombs (RGCHs), except for the thermal conduction properties of polycrystalline graphene-based carbon honeycombs (PGCHs).[10] Grain boundaries and grain size can influence the mechanical properties of nanocarbon materials significantly.[18–20] However, it is still unclear about the effect of grain size and cell irregularity on the mechanical properties of PGCHs. The related work not only reveals various natural phenomena, but also has enormous application prospects in the emerging field of nanotechnology.

    A comparative study of PGCHs and RGCHs can help us better understand their mechanical behavior and explore the related mechanism. Consider the cell in RGCHs as a grain. Its cell wall length is related to the grain size.[10] Meng et al.[7] found that the in-plane compression mechanical properties of RGCHs are mainly dependent on the grain size and the density of knots between graphene ribbons. Gu et al.[8] indicated that the mechanical properties of RGCHs under tension are dependent on the cell wall length. However, the cell wall length is less than ∼ 2.0 nm, and the compressive mechanical properties of RGCHs affected by the cell size are not reported. Zhang et al.[5] demonstrated in-plane tension and compression mechanical properties of RCHs with different cell wall lengths. Xing et al.[21] proposed anisotropic and tunable mechanical properties of asymmetric carbon honeycombs by constructing various cell wall sizes, found that the famous Gibson–Ashby model fails to predict the mechanical properties of RGCHs, and developed a new useful mechanical model. A systematic study is required on the grain size effect on the mechanical properties of RGCHs and the related mechanism, especially compared with the grain size effect on PGCHs.

    In this study, to study the effect of grain size and cell irregularity, a method based on Voronoi mosaic technology to construct the PGCHs is constructed for comparison and mechanism analysis. Then, based on molecular dynamics simulations (MDs), we systematically study the mechanical properties of in-plane and out-of-plane PGCHs under compression. We focus on the following questions: What are the effects of the average grain size and cellular irregularity of PGCHs on their mechanical properties?

2.   Methodology
  • The aperiodic structure of PGCHs is mainly realized by the Voronoi tessellation technique[10,22,23] with the Rhino software, which can construct random polycrystalline structures with various grain shapes. Figures 1(a)–1(c) show a typical geometry of RGCH with a zero-degree cellular irregularity. RGCHs are periodic arrays of honeycomb structures. The honeycomb wall is a single-layer graphene sheet (Fig. 1(a)). To form the honeycomb wall, the cell walls in the Voronoi diagram are replaced with armchair or zigzag-shaped graphene nanoribbons. The armchair junction is a six-membered ring structure (Fig. 1(e)), and the zigzag junction is a five–eight ring structure (Fig. 1(f)). The carbon atoms at the cell wall junction are marked in red (Figs. 1(e) and 1(f)). The cell structure of RGCHs is shown in Fig. 1(g). A parameter d (Fig. 1(d), not the h or l in Fig. 1(e)) is used to indicate the cell size for both PGCHs and RGCHs, which is the length between two seeds.[10] For RGCHs, there is a relation h=l=d/3 in the simulation models. For example, taking the grain size d = ∼ 1.0 nm in zigzag RGCHs as an example, the parameters h and l are about 0.58 nm. In the simulations, the grain sizes of PGCHs are chosen from the minimum size to about 10.0 nm, which can well present the varying trend due to the size effect. The minimum cell size stability in PGCHs with different cell irregularities is presented in Subsection 3.

    The random features of PGCHs are acquired by the Voronoi tessellation technique. First, a set of seeds is placed in space simultaneously and randomly. Second, these random seeds grow with a uniform velocity in all directions. Then, depending on the space dimension, a two-dimensional (2D) or 3D Voronoi diagram is constructed. The Voronoi tessellation structure is fully determined by the initial locations of the seeds. Using regularly positioned seeds produces regular Voronoi diagrams. In order to construct a honeycomb structure with irregular cell shapes, a regular hexagonal honeycomb structure with a perfectly ordered, regular cell shape, and uniform cell wall length is first constructed, as shown in Fig. 2(a). Then, perturbations are introduced to the reference model to generate Voronoi diagrams with irregular cell shapes and non-uniform cell wall length.

    The irregularity of cell shapes is determined by the irregular distribution of the seeds. The locations of the seeds used to construct Voronoi diagrams with irregular cell shapes are perturbed from a regular lattice of seeds. Figure 1(d) shows the coordinate perturbations of a regularly packed seed. The perturbed coordinates (xk, yk) of the seed k can be represented by

    where xk0 and yk0 are the two coordinates of the same seed in the regular lattice. d is the distance between two regularly packed (unperturbed) seeds. θk (∈ [0, 2π]) is a uniformly distributed stochastic angle between the x1-axis and the line connecting unperturbed and perturbed seeds. φk (∈ [−1, 1]) is a random variable with a uniform distribution. a is the amplitude used to quantify the degrees of cell shape irregularity, and ranges between 0 and 1. The smaller a is, the more regular the Voronoi diagram is. Regular hexagonal honeycombs are obtained when a = 0, and completely irregular honeycombs are defined when a = 1.0. Figures 2(e)–2(h) show honeycomb samples with different degrees of cell shape irregularity. In the simulations, the degree of cellular irregularity of random PGCHs is chosen as 0, 0.2, 0.4, and 0.65. Figures 2(a)–2(d) show four Voronoi diagrams of PGCHs with (a) a = 0, (b) a = 0.2, (c) a = 0.4, and (d) a = 0.65 degrees of cell irregularity (with an average grain size of 3.9 nm). Then, models of PGCHs with (e) a = 0, (f) a = 0.2, (g) a = 0.4, and (h) a = 0.65 degrees of cell irregularity are obtained (Figs. 2(e)–2(h)). Graphene-based cellular carbon presents various styles, including multi-walled porous nanocarbons and composite nanoporous carbons composed of other molecules and materials.[24,25] The connectivity between the pores is diverse and even non-existent. Here, we only discuss the ideal honeycomb structure with a mono-layer thickness.[1] More typical simulation models of PGCHs, with average grain sizes of 6.01 nm and 9.88 nm, are shown in supplementary information S1.

    The software package Lammps was used in the MD simulations. The structural analysis and processing were carried out by the visualization software OVITO. The binding interaction between the carbon atoms was described by the adaptive intermolecular reactive empirical bond order (AIREBO) potential.[26] The onset of the covalent interaction cut-off distance was set to 2.0 Å. The long-range van der Waals (vdW) interaction between carbon atoms was modelled by the Lennard–Jones potential with a well depth of 4.7483 × 10−22 J and an equilibrium distance of 0.3407 nm. The Nosé–Hoover thermostat was used to control the system temperature. The time step was taken as 1 fs.

    In the in-plane simulations (loaded in the x–y plane), the side lengths Lx and Ly of PGCHs and RGCHs in the x and y directions were both set to ∼ 60 nm, and the length Lz in the z direction was set to about 3.3 nm. Periodic boundary conditions were imposed in all three directions of RGCHs. Prior to the loading, the model was relaxed using the NPT ensemble until its energy was minimized at room temperature. Then an NVT ensemble was adopted to simulate the compressive behavior of PGCHs and RGCHs by applying a constant strain rate of 0.001 ps−1. Young’s moduli were calculated as the slope of the stress–strain curves E = σ/ε at a small strain of 0.5%. The energy absorption per unit volume Wv and energy absorption per unit mass Wm at a specific strain ε are defined respectively as follows:[6,21]

    where ρ is the mass density of GCHs.

    In the out-of-plane simulations (loaded in the z direction), the side lengths Lx and Ly of PGCHs and RGCHs in the x and y directions were both about 7 nm, and the length Lz in the z direction was about 10 nm. In the simulations, periodic boundary conditions were imposed in all three directions of RGCHs. In the calculation of the nominal stress of PGCHs and RGCHs, the cross-sectional area was defined as the product of the two side lengths in the x–y plane of PGCHs (Figs. 2(a)–2(d)). In the calculation of the real stress, the cross-sectional area was defined as the net area occupied by the graphene walls whose thicknesses were assumed to be 0.34 nm.

3.   Results and discussion
  • In symmetrical RGCHs, the cell wall height and length (h and l in Fig. 1(g)) equal h = l, and are different in asymmetric carbon honeycombs.[21] The Voronoi tessellation method in Section 2 can be used to construct any size of the height and length honeycomb cell wall. From the mathematical point of view, honeycomb with any small cell (grain) size is possible to build. However, physically, there are minimum cell (average grain) size for RGCHs and PGCHs, because that the cell walls of RGCHs and PGCHs are composed of graphene ribbons, and have minimum cell wall size h and minimum growth step sizes of cell wall Δh.

    For RGCHs with the cell irregularity degree a of 0 (see Eq. (1)), as shown in Fig. 3, the minimum cell sizes hminarm and hminzig for armchair and zigzag symmetrical RGCHs are about 0.49 nm and 0.58 nm, respectively.[6] Otherwise, cell walls with smaller sizes are not ideal graphene ribbons. As mentioned in Section 2, there is a relation h=l=d/3 between the cell wall and the average grain size d (Fig. 1(d)). Therefore, the corresponding minimum grain sizes dminarm and dminzig are ∼ 0.85 nm and ∼ 1.0 nm for armchair and zigzag RGCHs, respectively. In the following, we mainly use grain size d to describe PGCHs.

    The minimum average grain size of PGCHs is larger than dmin of RGCHs (PGCHs with a = 0). First, if the minimum average grain size of PGCHs is smaller than dmin of RGCHs, it means the cell wall does not consist of ideal graphene ribbons, because we already stated above that dmin is the smallest value for a cell wall to have ideal graphene ribbons. There should be some defects in the cell wall if the wall width is smaller than dmin, and it is not the armchair or zigzag honeycomb structure which is defined in Fig. 1. Second, non-zero cell irregularity will induce perturbation of the grain size. If the minimum average grain size of PGCHs is equal to dmin of RGCHs with 0 degree cell irregularity, some cell wall widths should be smaller than dmin, and some of them should be larger than dmin, because the average of them is equal to dmin. In the first case, we already stated that it is impossible for the minimum average grain size of PGCHs to be smaller than dmin of RGCHs. Therefore, the minimum average grain size of PGCHs is larger than dmin of RGCHs. In the following passage in this section, based on the analysis of the minimum grain size of RGCHs and the minimum growth step sizes of grain size, we will get the minimum average grain size dmin of PGCHs with 0.2, 0.4, and 0.65 cell irregularities.

    The minimum growth step sizes of grain size for armchair (zigzag) symmetrical RGCHs is Δdminarm≈0.43 (Δdminzig≈0.74) nm. The average grain size increases as d = dmin + n × Δdmin. Table 1 provides the cell wall size and average grain size of PGCHs with n from 0 to 7. As shown in Fig. 4, the grain size after variation based on dmin is

    where Δx and Δy are the coordinates variation of the grain size. Based on Eq. (1), we choose the maximum variable value of sinθk = ±1, cos θk = ±1, and φk = ±1. Then, we can get Eqs. (4a) and (4b) to predicate the grain size after maximum variation of armchair and zigzag PGCHs respectively

    For PGCHs with a = 0.2, using Eq. (4a), the grain size after variation of armchair PGCHs is dmin + Δd ≈ 1.24 nm. Therefore, the real minimum average grain size at least larger than 1.24 nm. Compared to Table 1, the real minimum average grain size should be 1.28 nm for armchair PGCHS with a = 0.2. Similarly, using Eq. (4b), the grain size after variation of zigzag PGCHs is dmin + Δd ≈ 1.46 nm. Compared to Table 1, the minimum average grain size should be 1.74 nm for zigzag PGCHS with a = 0.2.

    For PGCHs with a = 0.4, using Eq. (4a), the grain size after variation of armchair PGCHs is dmin + Δd ≈ 1.67 nm. Compared to Table 1, the minimum average grain size should be 1.71 nm for armchair PGCHs with a = 0.4. Similarly, using Eq. (4b), the grain size after variation of zigzag PGCHs is dmin + Δd ≈ 1.97 nm. Compared to Table 1, the minimum average grain size should be 2.48 nm for zigzag PGCHs with a = 0.4.

    For PGCHs with a = 0.65, using Eq. (4), the grain size after variation of armchair PGCHs is dmin + Δd ≈ 2.25 nm. Compared to Table 1, the minimum average grain size should be 2.57 nm for armchair PGCHs with a = 0.65. Similarly, using Eq. (4b), the grain size after variation of zigzag PGCHs is dmin + Δd ≈ 2.51 nm. Compared to Table 1, the minimum average grain size should be 3.21 nm for zigzag PGCHs with a = 0.65. For convenience, Table 2 shows the minimum cell wall size and minimum average grain size of RGCHs and PGCHs with 0, 0.2, 0.4, and 0.65 cell irregularities.

    As stated above, any small cell sizes of PGCHs are possible in mathematics based on the Voronoi tessellation method. We can contract PGCHs with smaller average grain size than the predicted minimum value. However, some cell walls in these conditions will not ideal graphene ribbons and have some defects. Take armchair PGCHs with 0.65 cell irregularity as an example. As shown in Fig. 5, we build a = 0.65 armchair PGCHs with 2.14-nm average grain size, which is smaller than the predicted minimum average grain size (2.57 nm) for armchair PGCHs with 0.65. As shown in Fig. 5, there are two types of defect walls. Type-I defect cell wall (Fig. 5(b)) is smaller than 0.25 nm. Type-II defect cell wall (Fig. 5(c)) is larger than 0.25 nm and smaller than 0.49 nm. Some defect walls may break after thermal relaxation and energy minimization. Even for the maintained structure stable, the cell wall structure is not PGCHs with ideal graphene ribbon cell wall. That is to say, it is not the ideal defined armchair or zigzag PGCHs in Fig. 1. Moreover, in the modeling process based on the Voronoi tessellation method, when one builds PGCHs with smaller average grain size and higher cell irregularity, more defects wall as shown in Fig. 5 will occur even if the building average grain size is larger than the critical value of the minimum average grain size. Therefore, to obtain ideal PGCHs with smaller average grain size and higher cell irregularity, more modeling iterations are required

  • The in-plane compression properties of honeycomb structures are a crucial concern in energy absorption in engineering design. Figure 6 shows the stress–strain curves of zigzag RGCHs and random PGCHs with different grain sizes under x-direction compression. The compression stress–strain curves of random PGCHs are consistent with those of RGCHs.[6,13,21] The stress–strain curves under x-direction compression show three ranges (Fig. 6): (I) the linear elastic stage, (II) the stress plateau stage, and (III) the densification stage. Compared to the macro-scale honeycomb, the densification stage in carbon honeycombs at the nano-scale actually includes an additional hardening stage due to the vdW interactions.[21,27] The detailed physical and mechanical significance of these stages can be seen in our previous results.[6,13,21] The zigzag RGCHs and random PGCHs with smaller grain sizes have higher compression stresses under the same strain (Fig. 6). The compression stress decreases with increasing grain size, and the overall trend of the compression stress curve of PGCHs shows a pseudo Hall–Petch relation.[21]

    The Young’s modulus, initial peak stress, mean plateau stress, and energy absorption per volume Wv in the linear elastic stage and plateau stage of zigzag RGCHs and random PGCHs decrease with increasing grain size (Figs. 7(a)–7(d)). As shown in Fig. 7(a), when the grain size increases from 1.0 nm to 9.8 nm, the Young’s modulus of the zigzag RGCHs with 0 cell irregularity decreases from about 222.1 GPa to 26.2 GPa. When the grain sizes increase from 3.9 nm to 10.0 nm, the Young’s modulus of zigzag random PGCHs with 0.2, 0.4, and 0.65 cell irregularities decreases from 38.3 GPa to 24.3 GPa, 27.6 GPa to 22.1 GPa, and 19.3 GPa to 17.2 GPa, respectively. As shown in Fig. 7(b), the initial peak stress of the zigzag RGCHs decreases from about 9.17 GPa to 0.51 GPa when the grain size increases from 1.0 nm to 9.8 nm. When the grain size increases from 3.9 nm to 10.0 nm, the initial peak stress of zigzag random PGCHs with 0.2, 0.4, and 0.65 cell irregularities decreases from 0.96 GPa to 0.42 GPa, 0.75 GPa to 0.33 GPa, and 0.31 GPa to 0.15 GPa, respectively. The smaller the grain sizes, the greater the density of the cell walls, which induces a more significant intensity of the vdW force between the cell walls. Hence, RGCHs and random PGCHs with a small grain size tend to have more tremendous stress under the same strain state.

    According to Gibson–Ashby continuum model, the Young’s modulus of honeycombs can be expressed as[21]

    where Ex and Ey are the Young’s modulus of honeycombs in the x- and y-directions, respectively, Eg is the Young’s modulus of the honeycomb composition material. Here, for RGCHs, the cell length and height is equal to h = l, the cell width t is ∼ 0.34 nm, and the angle is θ = 30°. Therefore, we have

    According to our new model,[21] the Young’s modulus of RGCHs in the x-direction and y-direction can be given by

    Substitution of h = l, the cell width t is ∼ 0.34 nm, and the angle is θ = 30° into Eq. (7) yields

    Using Gibson–Ashby model in Eq. (6) and our new model in Eq. (8) with Eg = 600 GPa,[6,20,21] we obtain the Young’s modulus of RGCHs as compared in Fig. 7(a). Both models indicate the Young’s modulus of RGCHs decrease with increasing cell size.

    Graphene and CHCs show brittle fracture behavior under external loading.[6,21] According to the Gibson–Ashby continuum model, the brittle fracture stress of honeycombs can be expressed as[21]

    where (σcr)x and (σcr)y are the fracture stresses of honeycombs in the x- and y-directions, respectively, σfg is the fracture stress of the honeycomb composition material. Substitution of the h = l, the cell width t is ∼ 0.34 nm, and the angle is θ = 30° into Eq. (11) yields

    According to our new model,[21] the fracture stresses of RGCHs in the x-direction and y-directions are

    Substitution of h = l, the cell width t is ∼ 0.34 nm, and the angle is θ = 30° into Eq. (10) yields

    Using the Gibson–Ashby model in Eq. (10) and our new model in Eq. (12) with σfg = 80 GPa,[6,20,21] we obtain the fracture stress of RGCHs compared with the initial peak stress in Fig. 7(b). Both models indicate that the initial peak stress of RGCHs decreases with increasing cell size.

    The mean plateau stress (Fig. 7(c)) and energy absorption per volume Wv (Fig. 7(d)) also decrease with increasing grain size over the whole varying trend. However, it should be noted that obvious fluctuations appear for random PGCHs, which may be due to the random and irregular grain structure. The mean plateau stress (Fig. 7(c)) and energy absorption per volume Wv (Fig. 7(d)) of PGCHs are higher than those of RGCHs. This means that random PGCHs can also be used as high-energy-absorption honeycomb materials.[6]

    Why do the mean plateau stress and energy absorption per volume Wv of RGCHs and PGCHs decrease significantly with increasing grain size? The variation trends in Wv and mean plateau stress are nearly consistent (Figs. 7(c)–7(d)). The Wv is mainly determined by the zone of mean plateau stress. The plateau stress reflects the bending or compressive buckling and failure of the cell walls in the whole honeycomb structure.[21] Short cell walls are more difficult to bend or buckle. Therefore, RGCHs with smaller grain size have higher plateau stress, and also have higher Wv.[21]

    Why are the mean plateau stress and energy absorption per volume Wv of PGCHs higher than those of RGCHs? The average plateau stress and energy absorption are determined by the total effect of all cell walls. For a single cell wall, the cell wall strength is related to the cell wall size by a negative first power relationship as Eq. (12), or a negative second power relationship as Eq. (10). With the same average cell (grain) size h, RGCHs have a h cell wall, and PGCHs have some smaller h – Δh and larger size h + Δh cell walls. Taking two cell walls and Eq. (12) as an example, the strength of RGCHs is

    and the strength of PGCHs

    Clearly, PGCHs have higher strength. Therefore, PGCHs have higher mean plateau stress and Wv than those of RGCHs. Theoretically, when the average grain size is the same, PGCHs with higher cell irregularity should have higher Wv. However, PGCHs in MD simulation are not infinite structures, and PGCHs with different degrees of cell irregularity under finite size cannot contain all random probabilities, so fluctuations of mean plateau stress Wv may occur (Figs. 7(c) and 7(d)).

  • The characteristic of the compression stress strain curves, Young’s modulus, initial peak stress, mean plateau stress, and energy absorption per volume Wv in the linear elastic stage and plateau stage of zigzag PGCH under y direction in-plane tension is similar to those of zigzag PGCH under x direction in-plane tension. The detail results can be seen in the supplementary information S2.

  • Figure 8 shows the stress–strain curves of zigzag RGCHs and random PGCHs with different grain sizes under z direction compression. Figure 8 can be divided into four distinct phases, namely the alignment elastic phase (phase I), the buckling phase (phase II), the structural failure phase (also known as the plateau phase III), and the densification phase (phase IV). The detailed physical and mechanical significance of these phases can be seen in our previous work.[6,13,21] The compression stress of zigzag RGCHs and random PGCHs decreases with the increase of the grain size. The mechanization is that the smaller the grain size of the PGCHs, the higher the density of the graphene wall, and the net area of the honeycomb cell wall increases, and it can withstand more significant compression stresses.

    In Fig. 9, the Young’s modulus, initial peak stress, mean plateau stress, and energy absorption per volume Wv of zigzag RGCHs and random PGCHs showed a decreasing trend with the increase of grain size. As shown in Fig. 9(a), the Young’s modulus of the zigzag RGCHs decreases from about 661.7 GPa to 52.3 GPa when the grain size increases from 1.0 nm to 9.8 nm. When the grain size increases from 3.9 nm to 10.0 nm, the Young’s modulus of zigzag random PGCHs with 0.2, 0.4, and 0.65 cell irregularities decreases from 142.1 GPa to 50.6 GPa, 157.8 GPa to 52.5 GPa, and 131.8 GPa to 35.1 GPa, respectively. As shown in Fig. 9(b), the initial peak stress of the zigzag RGCHs decreases from about 48.71 GPa to 1.25 GPa when the grain size increases from 1.0 nm to 9.8 nm. When the grain size increases from 3.9 nm to 10.0 nm, the initial peak stress of zigzag random PGCHs with 0.2, 0.4, and 0.65 cell irregularities decreases from 4.96 GPa to 1.01 GPa, 4.65 GPa to 0.99 GPa, and 3.23 GPa to 0.52 GPa, respectively. As shown in Fig. 9(c), the mean plateau stress of the zigzag RGCHs decreases from about 22.15 GPa to 0.52 GPa when the grain size increases from 1.0 nm to 9.8 nm. When the grain size increases from 3.9 nm to 10.0 nm, the mean plateau stress of zigzag random PGCHs with 0.2, 0.4, and 0.65 cell irregularities decreases from 2.03 GPa to 0.41 GPa, 2.0 GPa to 0.42 GPa, and 1.5 GPa to 0.29 GPa, respectively. As shown in Fig. 9(d), the Wv of the zigzag RGCHs decreases from about 10097.5 MJ/m3 to 289.6 MJ/m3 when the grain size increases from 1.0 nm to 9.8 nm. When the grain size increases from 3.9 nm to 10.0 nm, the Wv of zigzag random PGCHs with 0.2, 0.4, and 0.65 cell irregularities decreases from 1179.6 MJ/m3 to 221.8 MJ/m3, 1137.9 MJ/m3 to 223.9 MJ/m3, and 946.1 MJ/m3 to 174.6 MJ/m3, respectively.

    The effects of grain size and cell irregularity on the mechanical behavior of armchair RGCHs and random PGCHs can be seen in supplementary information S3. Armchair RGCHs and random PGCHs showed similar mechanical characteristics to the zigzag RGCHs and random PGCHs. Some deformation videos can be found in the attachments.

4.   Conclusions
  • Based on theoretical analysis and MD simulations, the minimum stable grain sizes in RGCHs and PGCHs are studied. The related mechanism is that, physically, RGCHs and PGCHs have a minimum cell wall size and minimum growth step sizes of the cell wall, because the cell walls are composed of graphene ribbons. The mechanical properties of RGCHs and PGCHs are investigated under compression. Under in-plane compression, the Young’s modulus, initial peak stress, mean plateau stress, and energy absorption decrease with increasing grain size overall, with some fluctuations. The mean plateau stress and energy absorption per volume of PGCHs are higher than those of RGCHs. Under out-of-plane compression, the Young’s modulus, initial peak stress, mean plateau stress, and energy absorption decrease with increasing grain size. The grain size effect is obvious, but the irregularity effect is weak. This research can help predict the performance of future RGCHs and random PGCHs in engineering applications.

Figure (9)  Table (2) Reference (27)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return