2026 Volume 35 Issue 1
Article Contents

Yu-Tong Chen, Jie-Ying Liu, Lan-Ying Zhou, Hua Yu, Tong Li, Qing Guan, Na Li, Yang Chai, Guang-Yu Zhang. Facile fabrication of twisted MoS2 bilayers by direct bonding[J]. Chinese Physics B, 2026, 35(1): 016803. doi: 10.1088/1674-1056/ae1c23
Citation: Yu-Tong Chen, Jie-Ying Liu, Lan-Ying Zhou, Hua Yu, Tong Li, Qing Guan, Na Li, Yang Chai, Guang-Yu Zhang. Facile fabrication of twisted MoS2 bilayers by direct bonding[J]. Chinese Physics B, 2026, 35(1): 016803. doi: 10.1088/1674-1056/ae1c23

Facile fabrication of twisted MoS2 bilayers by direct bonding

  • Received Date: 09/09/2025
    Accepted Date: 28/10/2025
    Available Online: 01/01/2026
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(4)

Article Metrics

Article views(378) PDF downloads(1) Cited by(0)

Access History

Facile fabrication of twisted MoS2 bilayers by direct bonding

Abstract: When stacking two-dimensional (2D) materials with a lattice mismatch and/or a small twist, moiré superlattice emerges with fascinating electronic and optical properties. The fabrication of such stacked 2D materials usually requires multiple transfer and stack processes, assisted by a certain transfer medium which needs to be removed afterwards, and it is very challenging to maintain pristine and clean surfaces/interfaces for these stacked structures. In this work, we report a facile direct bonding method for fabrication of twisted MoS2 bilayers with ultra-clean surfaces/interfaces. Novel interlayer interactions are revealed in the as-fabricated high-quality samples, leading to twist-angle related dispersion behavior of various Raman modes, such as layer breathing modes, shear modes and E2g modes, as well as indirect bandgap excitons. Field-effect transistors (FETs) of twisted MoS2 bilayers also exhibit angle-dependent performance, which could be attributed to the band structure evolution. This facile method holds significance for the future integration of pre-designed multilayer 2D materials and paves a way to explore underlying physical mechanisms and potential applications.

1.   Introduction
  • Two-dimensional (2D) moiré superlattice has given rise to a cornucopia of new phenomena, such as twist angle correlated electron states,[1,2] moiré excitons[3–5] and moiré phonons.[6,7] The most well-known 2D moiré superlattice is the magic-angle twisted bilayer graphene (TBG) recently demonstrated by Cao et al.[1] Fabrication of high-quality moiré system with precise twist angles is essential for the study of many intriguing physics. Generally, the fabrication of twisted 2D homo/heterostructures includes two strategies: direct growth and artificial stacking. While the former is constrained by thermodynamic mechanisms, the constituent materials are limited and they currently lack the capability for twist-angle control.[8–10] The latter applies to many different 2D materials and allows precise twist-angle control; but polymer supporting layers are usually involved during the transfer process, then contaminations such as polymer residues are inevitably present.[11–17]

    Recently, we demonstrated a direct wafer bonding method to realize wafer-scale stacked 2D homo/heterostructures without any involvement of polymer or chemical solution.[18] However, wafer-to-wafer alignment for precise twist-angle control remains an unsolved challenge and twist-angle dependent properties remain unaddressed for as-fabricated 2D homo/heterostructures. In this work, we report a direct bonding of single-crystalline monolayer MoS2 with hundred-micron domain sizes for twisted bilayers. A pre-alignment solution to the previous direct bonding method is developed, enabling twist angle control at a precision of ±0.2°. The as-fabricated twisted bilayer MoS2 (tb-MoS2) features ultra-clean and flat surface/interface, large-scale homogeneity, and strong interlayer coupling. The Raman fingerprint reveals the crystallographic reconstruction at small twist angles as well as engineering of indirect bandgap. The electrical measurements show an anomalously high mobility at the twist angle of 59.1°, which relates to the emergence of flat band in large moiré superlattice near 60°. This new fabrication method offers distinct advantages in the fabrication of precisely angular-controllable twisted homo/heterostructures, exhibiting unique optical evolution and electronic states.

2.   Method
  • The monolayer MoS2 we use is grown on sapphire substrate via oxygen-assisted chemical vapor deposition (O-CVD) as described in our previous works.[19,20] Controlling the growth time enables the growth of triangular large-grain monolayer MoS2 samples. The bonding process is performed in a glove box with water/oxygen concentration lower than 0.1 ppm. The bonding is conducted in a homemade apparatus, consisting of upper/lower flat plates. In the equipment, the hydraulic pressure module provides precise press force control (0–50000 N), and the temperature module controls the temperatures (20–500 °C) of both the upper and lower plates. During the bonding process, the temperature and pressure for both plates are 180 °C and ∼ 30 MPa, respectively. After pressure release, the bonded pair delaminates spontaneously, leaving as-fabricated tb-MoS2.

    To characterize the fabricated samples, Raman measurement is conducted on a Horiba LabRAM HR evolution Raman system with a 532 nm laser excitation. An 1800 lines/mm grating is used, providing a resolution of ∼ 0.7 cm−1. An ultra-low frequency (ULF) module is added for Raman measurements below 50 cm−1. The Raman spectrum is collected at 300 K in ambient atmosphere, and the photoluminescence (PL) spectrum at 300 K (78 K) is collected in ambient atmosphere (nitrogen atmosphere). Atomic force microscope (AFM) and piezoelectric force microscopy (PFM) imaging are performed by Bruker multimode 8 and Asylum cypher, respectively. Atomic-resolution high-angle annular dark-field (HAADF) scanning transmission electron microscope (STEM) images are acquired by the aberration-corrected JEM-ARM300F2 TEM operating at 300 kV.

    As for the fabrication of FET devices, the tb-MoS2 samples are transferred onto 20 nm Al2O3 dielectric layer via wet transfer method. After a standard ultraviolet (UV)-lithography patterning process, Au/Ti/Au electrodes are evaporated via an electron beam. Finally, the tb-MoS2 is patterned into ribbon channels by UV-lithography and plasma etching. The electrical measurement is conducted in a Janis 4-probe station by an Agilent B1500 semiconductor parameter analyzer.

3.   Results
  • Figure 1(a) illustrates the entire process including two steps: 1) pre-alignment and 2) direct bonding. The constituent MoS2 are triangular large-grain monolayer MoS2 grown on double-side polished (DSP) sapphire substrates (Fig. S1) by O-CVD. The triangular shape allows for orientation measurements under optical microscope during alignments, and transparent DSP sapphire enables a clear visualization when samples are viewed from its backside. The pre-alignment is realized using a transfer stage for precise twist-angle control. First, the back side of as-grown MoS2/sapphire samples are adhered onto the center of two bare sapphire wafers via transparent adhesive (Bisphenol-A polycarbonate, PC). The bottom sapphire base is fixed on the rotatable bottom stage, while the upper sapphire base is attached to the upper stage with a transparent polydimethylsiloxane (PDMS) film supported by a glass slide. Figure 1(b) shows the optical microscope image of upper (dotted yellow line) and lower (dotted dark-blue line) MoS2 triangles with a preset twist angle of 56.8°. After alignment, the glue (carbon tapes) that pre-adhered around the MoS2 pieces are brought into contact, fixing the sapphire pair. The PDMS film detaches from the upper sapphire base and then starts the bonding process.

    A typical as-fabricated tb-MoS2 sample is shown in Fig. 1(c) with the twist angle of 56.68° (the angle deviation δ ∼0.12°). More tb-MoS2 samples are shown in Fig. S2 and all the angle deviations are within 0.2°. In Table S1, we summarize angle deviations of typical transfer methods from previous results,[1,12,13,17,21,22] one can see that our method features one of the best alignment accuracies with considerably large size. These results reveal the effective angle control of our pre-alignment method. The holes and cracks in some samples are attributed to identical adhesion forces between two MoS2 films and their growth substrates. As shown in Fig. S3(a), the bonded pair includes three interfaces: two MoS2–sapphire interfaces and one MoS2–MoS2 interface. During debonding, the interface with the weakest adhesion forces delaminates. For bonding that uses two identical MoS2 films, i.e., fL1-substrate1 ≈ fL2-substrate2, as shown in Fig. S3(b), the competition between two identical adhesion forces leads to fragment of bonded bilayer MoS2 (Fig. S3(d)). This issue can be addressed by choosing samples with significant difference in adhesion forces (Fig. S3(c)), the resulting sample in Fig. S3(e) shows complete transfer of the overlapped MoS2 area.

  • Using this method, we fabricate a series of high-quality tb-MoS2 (Fig. S4), and the ultra-clean surfaces/interfaces are confirmed as follows. In a typical AFM image (Fig. 1(d)), the surface roughness is 0.047 nm, much flatter than that of samples fabricated by wet transfer method (0.519 nm) and pick-up dry transfer method (1.33 nm) as shown in Fig. S5. The clean interface leads to a strong interlayer coupling, as demonstrated by moiré patterns (Fig. S6) imaged by the PFM.[23] The moiré superlattice [24] in plane-view STEM images (Figs. S7 and S8) and interlayer spacing of 6.19 Å (close to the value in bulk MoS2) in cross-section (Fig. S9) HAADF-STEM image further provide direct evidence for strong-coupling in our samples.

    To further study the effect of interlayer coupling, we acquire Raman spectra on a 59.6° tb-MoS2 sample shown in Figs. 2(a) and 2(b). Two strong low-frequency interlayer vibration modes, i.e., layer breathing mode (LB) and shear mode (S), appear in Fig. 2(a), indicating a great interlayer coupling. These modes are fingerprints of well-coupled moiré superlattice and are sensitive to twist angles.[25] Figure 2(c) exhibits the corresponding spatial mapping of frequency and intensity of LB and S modes, respectively. The uniform distribution indicates large-scale homogeneity and twist-angle uniformity in our samples. The spatial mapping images of E2g and A1g mode from as-fabricated tb-MoS2 and as-grown 1L MoS2 are shown in Fig. S10, also revealing the uniformity of our samples.

  • In tb-MoS2, the twist angle can engineer the atomic reconstruction, in-plane strain distribution and optical band structure,[26] which can be reflected via Raman spectra. The moiré phonons exhibited in Fig. 3(a) are folded acoustic phonons under the modulation of periodic moiré potentials,[7,27] and vary with the twist angles. The evolution of moiré phonon is determined by moiré period λ (λ = a/[2sin (θ/2)], where a is the lattice constant of MoS2). By calculating the phonon dispersion with respect to the reciprocal lattice vector g[7,28–30] (see details in Fig. S11), we obtain the evolution of folded longitudinal acoustic (FLA) and folded transverse acoustic (FTA) as a function of the twist angle (calculated FLA and FTA in Fig. 3(c)). FLA and FTA extracted from Fig. 3(a) fit well with calculated results, demonstrating the high quality of our samples.

    Previous studies on tb-MoS2 reveal a transition from rigid lattice to relaxed lattice when the twist angle decreases to near 0°.[23,31,32] This transition is also observed in our samples. As shown in Figs. 3(b) and 3(d), S mode appears and LB mode shows a sudden blue shift when twist angle θ is less than 4.9°. This phenomenon is attributed to the formation of reconstructed region that contributes to the emergence of the S mode with enhanced restoring force. These behaviors indicate the transition from rigid regime (θ > 4.9°) to relaxed regime (0 < θ < 2°).[31]

    In the relaxed regime, the full width at half maximum (FWHM) of S mode (Fig. 3(f)) undergoes a rapid decrease from 0° to 2°, originating from the decreased in-plane strain that reduces the strain-induced splitting effect of the doubly degenerate S mode.[33] The reduced strain is also verified by similar behavior in the FWHM of E2g mode (Fig. 3(f), the full spectra is shown in Fig. S12). In the relaxed regime, the moiré superlattice consists mainly of the MX′/X′M-stacking domains that are more energetically-favored,[31] verified by our PFM results of large MX′/X′M domains. As the moiré period undergoes a large drop from 0° to 2° (Fig. S13), the MX′/X′M domain area decreases, and the in-plane strain is also modulated. When θ > 2°, the moiré period is less than 10 nm, the strain among superlattice gradually becomes stable, and FWHM of S mode and E2g remain unchanged,[31] referred to as the intermediate regime. As for LB mode, the FWHM increases as twist angle increases from 0° to 4.9° (Fig. 3(f)) along with a rapid frequency red shift at 4.9°, indicating a splitting here due to phonon-phonon coupling.[31] When θ > 4.9°, the unchanged frequency and FWHM of LB mode indicate a stable rigid-superlattice.

    PL spectrum also reveals the twist-angle dependent optical band structure (Figs. 3(e) and S14). As shown in the inset in Fig. 3(e), MoS2 undergoes a transition from direct bandgap to indirect bandgap from monolayer to bilayer, with the appearance of indirect bandgap exciton. Figure 3(e) summarizes the positions of excitons as a function of the twist angle. Please also refer to Fig. S14 for low-temperature PL spectrum. The indirect bandgap exciton shows blue shift from 1.35 eV (∼0°) to 1.58 eV (∼30°), and shifts to 1.5 eV when the angle reaches higher; while the positions of A and B excitons remain nearly unchanged, in agreement with previous results.[13,34]

  • The electrical properties of tb-MoS2 at different twist angles ranging from 0° to 60° are also investigated. The schematic device structure is shown in the inset in Fig. 4(a). The output curves (Fig. 4(a)) from a typical 59.1° tb-MoS2 device exhibit linear behavior, suggesting an ohmic contact. Figure 4(b) shows the transfer curve from the same device and the on/off ratio reaches 107. The average field-effect mobility is summarized in Fig. 4(c), and it can be seen that the mobility slightly drops at around 10°/51.6° and reaches a maximum value of ∼50 cm2⋅V−1⋅s−1 at 59.1°. The high mobility near 60° can be attributed to high density of states from the flat electronic band.[35–37]

4.   Conclusion
  • We report a direct bonding method with precise angular alignment to fabricate large-scale, ultra-clean, uniform and high-quality tb-MoS2 with a twist angle accuracy of 0.2°. In our as-fabricated samples, twist-angle dependent behavior of moiré phonons, interlayer vibration modes, and indirect bandgap are studied, revealing the evolution of superlattice, in-plane strain, as well as optical band structure. We also fabricate electrical devices with various twist angles and find signature of flat band near 60°. Our work provides a facile method to fabricate a moiré system and could pave a way for moiré physics and emerging applications.

Figure (4)  Reference (37)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return