White light-emitting diodes (WLEDs) are among the most prominent solid-state lighting and display technologies due to their high efficiency, energy savings, environmental friendliness, and long operational lifetime.[1–5] The performance of phosphor-converted WLEDs is largely determined by the luminous efficiency, thermal stability, and spectral characteristics of the employed phosphor materials.[1,6] In recent years, the development of novel phosphors with outstanding overall performance has become a major research focus. Among various luminescent hosts, molybdate-based materials have attracted considerable attention due to their structural diversity, robust physicochemical stability, and relatively mild synthesis conditions.[7,8]
Terbium ions (Tb3+) are widely recognized as an important green-emitting activator in WLEDs. Their intense, narrow-band green emission, originating from the characteristic 5D4 → 7F5 transition, is essential for achieving a high color rendering index.[9–11] However, a common issue in conventional Tb3+-doped phosphors is concentration quenching, where the emission intensity decreases upon exceeding a critical dopant concentration.[12,13] This behavior has been widely reported in various host matrices. For example, in oxide hosts such as Y2O3, the quenching concentration typically falls between 5 at% and 8 at%, primarily due to energy migration via dipole–dipole interactions.[14] Phosphate-based hosts often exhibit an even lower critical concentration, around 1 at%; in LiMgPO4, for instance, Tb3+ doping beyond 1.5 at% leads to a pronounced drop in emission intensity.[15] Therefore, the development of Tb3+-doped systems that resist concentration quenching and maintain high emission efficiency even at high or complete doping levels is of substantial scientific and practical importance.
KBi(MoO4)2 (abbreviated as KBM), a molybdate host with a layered crystal structure, offers a unique platform to investigate the doping behavior of Tb3+ ions.[16,17] In this work, we systematically explored the structural evolution, luminescence properties, and energy transfer mechanisms of Tb3+ in KBM across the full concentration range, from undoped (0 at%) to complete substitution of Bi3+ by Tb3+ (100 at%, yielding KTb(MoO4)2, abbreviated as KTM). Remarkably, the KBM: xTb3+ system exhibits an anomalous anti-concentration quenching phenomenon: the luminescence intensity increases monotonically with Tb3+ content from 0% to 100%, and shows no conventional quenching plateau or decline. Detailed analysis reveals that this behavior arises from the unusually large Tb3+–Tb3+ separation (> 5 Å) afforded by the quasi-layered crystal structure, which effectively suppresses multipolar-interaction-mediated energy migration. At full Tb3+ substitution, the material undergoes a structural phase transition from the monoclinic KBM to the triclinic α-KTM, accompanied by a shift in luminescence mechanism. Furthermore, the system demonstrates excellent thermal and cycling stability.
-
The Tb3+-doped KBi(MoO4)2 (KBM) samples were synthesized via a high-temperature solid-state reaction method. High-purity reagents, including K2CO3 (99.9%), Bi2O5 (99.99%), MoO3 (99.9%), and Tb2O3 (99.9%) from Aladdin, were used as starting materials. The doping concentrations of Tb3+ ions in the KBM host were selected as 0 at%, 10 at%, 30 at%, 50 at%, 70 at%, and 100 at%. The raw materials were accurately weighed according to the stoichiometric ratio, then were mixed in an agate mortar and ground for 30 min. The thoroughly ground mixture was transferred into a crucible and placed in a muffle furnace. The temperature was gradually increased to 600 °C over a period of 4 hours and maintained at this temperature for 12 hours to ensure complete reaction. Afterward, the sample was cooled to room temperature. Finally, the synthesized samples were ground again for further characterization.
-
Phase structural analysis was performed using a Bruker D8 Advance x-ray diffractometer (XRD) equipped with Cu-Kα radiation (wavelength λ = 1.5406 Å). Scanning was conducted in continuous mode over a 2θ angle range of 10°–80°, with a step size of 0.02°. The morphology and elemental distribution of the samples were characterized using a JSM-6510 scanning electron microscope (SEM). The excitation spectra, emission spectra and fluorescence decay curves were obtained using an Edinburgh FLSP-920 spectrometer, fitted with a xenon lamp as the excitation source. The temperature-dependent spectra were recorded by the same spectrometer equipped with a Lake Shore 355 temperature controller with a precision of ±0.5 K.
2.1. Preparation of samples
2.2. Characterizations
-
To comprehensively investigate the phase purity and structural characteristics of the samples, we performed x-ray diffraction (XRD) analysis followed by Rietveld refinement. Figure 1(a) displays the XRD patterns of Tb3+-doped KBM samples with doping concentrations ranging from 0% to 70%. Since no standard reference pattern is available for KBM, the standard pattern of RbBi(MoO4)2 (RBM) (ICSD #4181) was adopted as a reference. This decision is based on the similarity in crystal structure and electronic configurations between K and Rb, both alkali metals in the same group of the periodic table. Consequently, the XRD pattern of RBM was employed for structural analysis and phase identification of KBM. The XRD results indicate that the patterns of x Tb3+-doped KBM samples (KBM: xTb3+) closely match the reference pattern, demonstrating that Tb3+ successfully substitutes for Bi3+ at the lattice sites within the KBM: xTb3+ system. Furthermore, the XRD patterns exhibit a significant angular shift in diffraction peaks as the Tb3+ doping concentration increases. This phenomenon can be attributed to the noticeable difference in ionic radii between Tb3+ and Bi3+. The ionic radius of Tb3+ (CN = 8, R = 1.04 Å) is smaller than that of Bi3+ (CN = 8, R = 1.17 Å). According to Bragg’s law, the substitution of the smaller Tb3+ ion reduces the interplanar spacing (d), resulting in an increased diffraction angle (2θ), and thus, a shift of the diffraction peaks toward higher angles.
Figure 1(b) shows the XRD pattern of KTM, which is formed by the complete substitution of Bi3+ with Tb3+ at 100% doping concentration. The XRD analysis reveals that the diffraction patterns of the synthesized KTM samples closely align with the α-KTM reference spectra in terms of peak positions and relative intensities. However, the patterns deviate significantly from both KBM and β-KTM, confirming a structural transformation at 100% Tb3+ doping. Specifically, the monoclinic KBM phase (space group P21) transitions to the triclinic α-KTM phase (space group P1) upon full substitution of Bi3+ by Tb3+.[18,19]
Additionally, the Rietveld refinement of KBM: 10 at% Tb3+ (Fig. 1(c)) reveals that, at doping concentrations below 100%, the crystal structure of KBM remains unchanged and maintains its original monoclinic structure. Figure 1(d) presents the Raman spectra of KTM and KBM. Analysis of the Raman peaks reveals high consistency between the KTM and KBM samples in the middle- and high-frequency regions. However, in the low-frequency domain, the Raman peaks of KTM are predominantly centered at 137 cm−1, 104 cm−1, and 65 cm−1, while those of KBM are located at 140 cm−1 and 75 cm−1.[20,21] Since phonon energy (E) is directly proportional to vibrational frequency (v) via the relation E = hv,[22] this comparison indicates that KTM exhibits lower phonon energies than KBM in the low-frequency region. This structural transformation may be attributed to lattice distortion, which occurs as the smaller Tb3+ ions replace the larger Bi3+ ions, causing a shift from the monoclinic to the triclinic phase, as depicted in Fig. 1(e).[23] Figure 1(f) presents the SEM and elemental mapping results of KBM: xTb3+, demonstrating a homogeneous distribution of Tb3+ across the constituent elements (K, Bi, Mo, and O), confirming the uniform doping of Tb3+ within the KBM matrix.
-
We measured the luminescence spectra of KTM and KBM: xTb3+ phosphors and systematically investigated their luminescence properties. Figure 2(a) illustrates the excitation spectra of the KTM phosphor at room temperature. At the monitoring wavelength of 550 nm, a broadband absorption spanning 280–330 nm with a maximum value at 308 nm is clearly observed, corresponding to the charge transfer band (CTB) of the [MoO4]2− group.[24] In the 330–400 nm range, multiple excitation peaks were observed, which are attributed to the characteristic absorption transitions of Tb3+. These peaks correspond to the characteristic wavelengths of 360 nm (7F6 → 5D2), 370 nm (7F6 → 5D4+5L9), 380 nm (7F6 → 5G5), 390 nm (7F6 → 5L10), and 398 nm (7F6 → 5G6+5D3), respectively.[25] We compared the excitation characteristics of KTM and KBM: 30 at% Tb3+ phosphors in the range of 260–360 nm, as shown in Fig. 2(b). Despite the differences in emission intensity at different excitation wavelengths, both KTM and KBM: 30 at% Tb3+ show a strong absorption response under 305 nm laser excitation. It is noteworthy that the excitation spectra of KBM: 30 at% Tb3+ contain characteristic absorption transitions of Bi3+ ions under weak crystal field (1S0 → 3P1) and [MoO4]2− charge transfer transition, whose peaks are located at 280 nm and 320 nm, respectively.[26,27] Whereas KTM has only [MoO4]2− charge transition absorption under 305 nm excitation.
To further analyze the photoluminescence properties of the KBM: 30 at% Tb3+ phosphor, Fig. 2(c) shows the normalized emission spectra under different excitation wavelengths. Excitation wavelengths of 280 nm, 305 nm, and 379 nm were selected, corresponding to spectral lines depicted in blue, orange, and green, respectively. The results indicate that the positions of the emission peaks remained largely unchanged across different excitation wavelengths. Within the range of 450–700 nm, the most prominent emission peaks were observed at 480 nm, 545 nm, 580 nm, and 630 nm. These peaks correspond to the transitions from the 5D4 energy level of Tb3+ ions to the 7F6, 7F5, 7F4, and 7F3 energy levels, respectively.[28] We investigated the emission behavior of KBM phosphors with varying Tb3+ doping concentrations (x = 0 at%, 10 at%, 30 at%, 50 at%, 70 at%, 100 at%) under 305 nm and 379 nm excitation, as shown in Figs. 2(d) and 2(e). The emission intensity increased monotonically with Tb3+ concentration, reaching a maximum at x = 100 at%. Characteristic emission peaks were observed in the 450–700 nm range, with dominant peaks at 480 nm, 545 nm, 580 nm, and 625 nm, along with weak peaks at 650 nm, 670 nm, and 680 nm. All peaks correspond to the characteristic 5D4 → 7FJ (J = 6, 5, 4, 3, 2, 1, 0) transitions of Tb3+ ions.[25] In investigating the effect of Tb3+ doping concentration on emission intensity, we observed a distinctive phenomenon. As depicted in Fig. 2(f), the normalized emission intensity increases continuously as the Tb3+ concentration rises from 0 at% to 100 at%, irrespective of excitation at 305 nm. This contrasts with typical concentration quenching behavior reported for fluorescent materials, where luminescence intensity plateaus or declines beyond a critical dopant concentration due to inter-ionic energy transfer and non-radiative transitions.[29,30] Remarkably, our samples exhibit persistent emission enhancement across the entire doping range (0–100 at%) without evidence of concentration quenching. The underlying mechanisms for this anomalous behavior will be analyzed in the following contents.
The color coordinate diagram and CIE chromaticity coordinate serve as core parameters for evaluating phosphor luminescence characteristics. Figure 2(g) displays the CIE coordinates of KBM: xTb3+ phosphors under 305 nm excitation. Increasing Tb3+ doping concentration induces a progressive shift of the color coordinates toward the green region in the chromaticity diagram. The upper-right inset contrasts KTM samples under daylight versus 305 nm excitation, exhibiting distinct green emission under 305 nm excitation. Furthermore, comparison of emission spectra for KTM and KBM: 50 at% Tb3+ under both 305 nm and 379 nm excitation (Fig. 2(h)) reveals consistent spectral profiles and emission colors aligned with CIE analysis. All observed peaks correspond to characteristic Tb3+ transitions, which indicates the existence of an energy transfer process.
Additionally, as shown in Fig. 2(g), increasing Tb3+ doping concentration induces a systematic shift of color coordinates in the CIE chromaticity diagram from initial yellow-green toward the lime-green region. Although modest in magnitude, this shift exhibits excellent linearity. To quantify this trend, we performed linear fitting of the CIE y-coordinate, yielding the following equation:
The fitting results reveal a strong linear correlation between Tb3+ concentration (x) and the CIE y-coordinate as shown in Fig. 2(i), with each concentration x uniquely determining both the y-value and corresponding emission color. This precise correspondence allows establishing a comprehensive CIE chromaticity database over the studied concentration range. Thus, for anti-counterfeiting applications, precisely designed concentration gradients can create high-dimensional security codes that exhibit continuous color gradients under UV illumination.
-
To elucidate the intrinsic mechanism underlying the anti-concentration quenching phenomenon observed in doped samples, we conducted an in-depth investigation into their crystal structures and energy transfer. Generally, the concentration quenching phenomenon is closely associated with energy transfer between activator ions, where energy migrates from one activator ion to another and eventually reaches lattice defects or quenching centers.[6] This indicates that the absence of concentration quenching in KBM: xTb3+ materials may be attributed to inefficient energy transfer among Tb3+–Tb3+ ions. As reported in Blasse’s study,[31] exchange interactions dominate the energy transfer process when the ion spacing is below 5 Å, whereas multipolar interactions prevail when the spacing exceeds 5 Å. Notably, the contribution from multipolar interactions to energy transfer is significantly weaker than that from exchange interactions. As shown in Fig. 3(a), both monoclinic KBM and triclinic α-KTM exhibit layered crystal structures, where K+ ions connect adjacent layers through ionic bonds. The large ionic radius of K+ not only spatially separates Bi3+ and Tb3+ into different atomic layers but also significantly expands the interlayer spacing. This structural characteristic significantly increases the inter-ionic distance between activator ions. Based on the above structural characteristics, we calculated the Tb3+–Tb3+ distances in KBM:10 at% Tb3+ and KTM using the following equations:[32]
where Xc denotes the critical concentration, N is the number of cations per unit cell, and V represents the unit cell volume. In the KBM: xTb3+ materials, the Tb3+–Tb3+ distances were calculated for critical concentrations (Xc) of both 10 at% and 100 at%, given the absence of observable concentration quenching. For Xc = 10%, substituting V = 635.563 Å3 and N = 4 into the equation yields a Tb3+–Tb3+ distance of 14 Å. At Xc = 100% (with V = 662.015 Å3 and N = 2), the calculated distance decreases to 6 Å. These results demonstrate that the Tb3+–Tb3+ separation remains above 5 Å even at the maximum doping concentration of 100 at%. According to energy transfer theory, multipolar interactions become dominant in this case, effectively suppressing both cross-relaxation and resonance energy transfer processes, thereby significantly reducing the probability of concentration quenching.[31] Meanwhile, the absence of concentration quenching is linked to the distinctive electronic structure of Tb3+ ions. The 4f electron orbitals are effectively shielded by the outer 5s25p6 electron shells, which dramatically weakens their interaction with neighboring ions or lattice defects.[33] This shielding effect consequently suppresses nonradiative transitions that would otherwise lead to concentration quenching. Thus, this shielding effect suppresses the occurrence of non-radiative transitions, consequently giving rise to the phenomenon of anti-concentration quenching. Furthermore, the substantial energy gap between Tb3+ ground state (7F6) and excited state (5D4) not only reduces energy transfer probability but also markedly weakens electron–phonon coupling, thereby further suppressing the concentration quenching mechanism.[33]
The emission spectra of the undoped and low-Tb3+-doped (< 15%) samples, together with the KTM sample, are shown in Fig. 3(b). It is evident that the undoped sample exhibits a pronounced broadband emission near 470 nm (in clear contrast to the Bi3+-free KTM sample), which is assigned to the intrinsic Bi3+ 3P1 → 1S transition. Notably, the intrinsic Bi3+ emission progressively weakens with increasing Tb3+ concentration, indicating resonant energy transfer between Bi3+ and Tb3+; the proposed transfer mechanism is depicted in Fig. 3(c). At low doping concentrations (x < 100 at%), energy transfer from both Bi3+ (1S → 3P1 under 280 nm excitation) and [MoO4]2− (1A1 → 1T2 under 305 nm excitation) sensitizes the 5D3 level of Tb3+. Concurrently, Tb3+ directly absorbs 379 nm photons (via 7F6 → 5D3 transition).[34–36] Subsequently, electrons in the 5D3 level undergo non-radiative relaxation to the 5D4 level. Ultimately, the 5D4 excited electrons transition to the ground states (7F6 → 7F), activating characteristic Tb3+ emissions through radiative transitions that produce distinct wavelength bands and corresponding colors. At 100 at% Tb3+ doping concentration, complete replacement of Bi3+ sites by Tb3+ shifts the luminescence mechanism to a [MoO4]2−-Tb3+ synergistic system. Here, [MoO4]2−-mediated energy transfer (following UV absorption) cooperates with direct Tb3+ excitation to jointly drive the characteristic emissions. This concentration-dependent mechanism transition provides a fundamental basis for designing multimodal anti-counterfeiting materials.
-
To further investigate the properties of the phosphor samples, we compared the temperature-dependent luminescence of KBM: 50 at% Tb3+ and KTM over the range of 300 K to 440 K, as shown in Fig. 4(a). The luminescence intensity of both KBM: 50 at% Tb3+ and KTM gradually decreases as temperature increases, a behavior that manifests characteristic thermal quenching. The thermal quenching mechanism can be primarily attributed to enhanced lattice vibrations at elevated temperatures, which induce the formation of Urbach tail states through the tail of electronic state distribution from the conduction band edge into the bandgap.[37] These tail states effectively overlap with the excited energy levels (5D4 and 5D3) of Tb3+ ions, providing a nonradiative relaxation pathway where excited electrons can transition to the conduction band rather than returning to the ground state through radiative emission. In the low-frequency range, KBM: xTb3+ exhibits higher phonon energy than KTM at doping concentrations below 100%. This energy difference reduces the thermal quenching effect, which leads to a more gradual intensity decay, due to the fact that higher phonon energies may accelerate the non-radiative relaxation by promoting phonon–electron coupling, thus exacerbating the thermal quenching.[38] Furthermore, we examined the 2D temperature-dependent emission spectra of KBM: 50 at% Tb3+ and KTM under 379 nm excitation (Fig. 4(b)). Similar to the 305 nm excitation case, the characteristic Tb3+ emission peaks are observed, and their positions show no significant temperature shift. This further demonstrates that the crystal-field environment around Tb3+ in the host remains stable.
To deeply investigate the thermal stability of KTM and KBM: 50 at% Tb3+, we performed thermal cycling tests on both phosphors (Fig. 4(c)). Under 379 nm excitation, the temperature underwent five complete cycles, each consisting of heating from 300 K to 440 K followed by cooling back to 300 K. To facilitate direct comparison of cycling stability, the luminescence intensity was normalized, as shown in Fig. 4(d). The results demonstrate that both materials exhibit excellent stability and repeatability.
The luminescence thermal stability discrepancy between KBM: 50 at% Tb3+ and KTM was quantitatively characterized by normalizing their temperature-dependent luminescence intensities over the 300–440 K range (Figs. 4(e) and 4(f)). Experimental data reveal that while both materials exhibit typical thermal quenching behavior, KTM demonstrates notably superior luminescence thermal stability compared to KBM: 50 at% Tb3+ under both 305 nm and 379 nm excitation. Specifically, KTM retains 63.2% of its initial luminescence intensity at 360 K under 305 nm excitation. This divergence stems from distinct local environments of Tb3+ ions: in the KTM host, Tb3+ occupies intrinsic lattice sites with optimal charge matching to host cations, establishing a uniform crystal field.[39] This configuration minimizes high-temperature lattice distortion and mitigates perturbation of Tb3+ excited states. By contrast, in the KBM: 50 at% Tb3+ system, Tb3+ substitutes for Bi3+ as a dopant ion. The significant ionic radius difference between Bi3+ and Tb3+ triggers lattice distortion, leading to inhomogeneous crystal field distribution around Tb3+. As temperature increases, thermal vibrations amplify this distortion, promoting coupling between Tb3+ excited states and phonons. This enhances non-radiative transition rates, ultimately manifesting as accelerated luminescence decay.[40]
-
To further investigate the thermal stability properties of the phosphors, we applied the Arrhenius equation to determine activation energies and analyze their thermal quenching behaviors:[41]
where I0 and I(T) are the initial and temperature-dependent emission intensities, respectively. Ea refers to the thermal quenching activation energy, A is a constant, and k is the Boltzmann constant (8.62 × 10−5 eV/K). Figure 5(a) presents the thermal quenching activation energies Ea of KBM: 50 at% Tb3+ (0.4059 eV) and KTM (0.6129 eV). KTM exhibits a significantly higher activation energy than KBM: 50 at% Tb3+, consistent with the conclusion of temperature-dependent luminescence characteristics of both phosphor materials in the preceding section. Notably, both phosphors exhibit substantially higher Ea than typical Tb3+-doped materials, as shown in Table 1, confirming their exceptional thermal stability.
To delve deeper into the luminescence mechanism of the phosphors, we systematically investigated the fluorescence decay lifetimes of KBM: xTb3+ (x = 10 at%, 30 at%, 50 at%, 70 at% and 100 at%) phosphors with varying Tb3+ doping concentrations, as presented in Figs. 5(b) and 5(c). Notably, the fluorescence decay curve of the KTM sample follows a single-exponential decay model, yielding a fluorescence decay lifetime of 0.529 ms after fitting.[46] This behavior indicates that only one luminescence center for Tb3+ exists in the KTM host. However, KBM: xTb3+ (x = 10 at%, 30 at%, 50 at% and 70 at%) whose fluorescence decay was fitted with a double-exponential function[47]
where components τ1 (fast decay) and τ2 (slow decay) demonstrate concentration-dependent evolution. As the doping concentration of Tb3+ increases from 10 at% to 70 at%, the value of τ1 increases from 0.013 ms to 0.103 ms, and the value of τ2 increases from 0.383 ms to 0.467 ms. These distinct fluorescence lifetime decay behaviors are closely related to their crystal structures and energy transfer mechanisms, as shown in Fig. 5(d). In KTM host, Tb3+ ions occupied intrinsic lattice sites within a uniform crystal field distribution. The [MoO4]2− groups absorb energy and efficiently transfer it to adjacent Tb3+ ions via a singular pathway. On the other hand, KBM: xTb3+ manifests dual luminescent centers of Bi3+ and Tb3+. In addition, the doping of Tb3+ leads to lattice distortion and inhomogeneous crystal field distribution, which complicates the energy transfer paths. Specifically, the energy absorbed by Bi3+ ions is then transferred to Tb3+ via the ET-1 path, and the energy absorbed by [MoO4]2− groups is transferred to Tb3+ via the ET-2 path. In summary, the differences in host structures lead to divergent luminescent behaviors: the KTM host has only one luminescent center and the KBM: Tb3+ hosts have dual centers. These structural distinctions directly manifest as single exponential versus double-exponential fluorescence decay behaviors, elucidating fundamental mechanistic divergences between these phosphors.
To elucidate the temperature-dependent luminescence characteristics of the phosphors, the fluorescence lifetimes of KTM and KBM: 50 at% Tb3+ phosphors were probed across distinct temperature ranges. Figures 6(a) and 6(b) depict the fluorescence decay curves of KTM samples within the temperature intervals of 300–360 K and 380–440 K, respectively. Fitting analysis reveals that within the 300–360 K range, the fluorescence lifetime of KTM undergoes a gradual transition from 0.529 ms to 0.375 ms, and the decay behavior is amenable to single exponential function fitting. As the temperature increases to the 380–440 K range, the fluorescence decay manifests a double-exponential feature. This single exponential to double-exponential decay mode shift can be attributed to thermally-induced lattice distortion. The high temperature intensifies the lattice thermal vibration, which changes the crystal field environment of some Tb3+ ions and splits the excited state energy levels, resulting in some ions being in a strongly coupled environment and others in a weakly coupled environment.[39] When the temperature reaches 380 K, the phonon–electron coupling is significantly enhanced, which activates the non-radiative transition channels and leads to phonon-assisted energy transfer between ions. Ultimately, this culminates in the fluorescence decay behavior evolving from single exponential to double exponentials. We systematically studied the temperature-dependent fluorescence lifetime properties of KBM: 50 at% Tb3+ and KTM phosphors as shown in Figs. 6(c) and 6(d). The experimental results demonstrate that between 300 K and 440 K, KBM: 50 at% Tb3+ consistently displays double-exponential fluorescence decay behavior. The fast decay component τ1 represents the energy transfer from Bi3+ to Tb3+, while the slow decay component τ2 corresponds to direct excitation from [MoO4]2− to Tb3+.[20,27,33] Both lifetime components decrease with rising temperature. Specifically, τ1 reduces from 0.429 ms to 0.034 ms, suggesting the energy transfer efficiency between Bi3+ and Tb3+ declines due to stronger lattice vibrations. Meanwhile, τ2 shortens from 0.077 ms to 0.004 ms, mainly caused by enhanced multi-phonon non-radiative relaxation at elevated temperatures. In comparison, KTM exhibits single-exponential decay characteristics, indicating it contains only one luminescent center.
3.1. Structure analysis
3.2. Luminescence properties
3.3. Anti-concentration quenching mechanism
3.4. Luminescence thermal stability
3.5. Fluorescence decay properties
-
In this work, KBM: Tb3+ phosphors were synthesized via high-temperature solid-state reaction, with their luminescence properties systematically characterized across a wide doping range (0–100 at% Tb3+). Remarkably, these materials demonstrate an unusual anti-concentration quenching effect, where luminescence intensity increases monotonically with Tb3+ concentration. This distinctive behavior originates from the large interionic distances (> 5 Å) between Tb3+ ions in the layered crystal structure, which effectively suppresses energy migration through multipole interactions. Complete substitution of Bi3+ with Tb3+ (100 at%) induces a structural phase transition from monoclinic to triclinic (α-KTM), exhibiting superior thermal stability (activation energy = 0.6129 eV). Precise control of Tb3+ doping concentration enables linear tuning of CIE chromaticity coordinates, suggesting potential applications in anti-counterfeiting technologies. Fluorescence lifetime analysis reveals mono-exponential decay for α-KTM, contrasting with the bi-exponential behavior observed at intermediate doping levels. These findings provide valuable insights for developing advanced rare-earth doped phosphors with applications in solid-state lighting and security marking.