2026 Volume 35 Issue 2
Article Contents

Shaozheng Wang, Xumin Chang, Feng Liu, Yuchen Zheng, Juncai Wu, Tong Zheng, Kenji Watanabe, Takashi Taniguchi, Shengwei Jiang. Charge-transfer-induced re-entrant ferromagnetism in twisted-bilayer-MoTe2/hBN/WSe2[J]. Chinese Physics B, 2026, 35(2): 027101. doi: 10.1088/1674-1056/ae1c27
Citation: Shaozheng Wang, Xumin Chang, Feng Liu, Yuchen Zheng, Juncai Wu, Tong Zheng, Kenji Watanabe, Takashi Taniguchi, Shengwei Jiang. Charge-transfer-induced re-entrant ferromagnetism in twisted-bilayer-MoTe2/hBN/WSe2[J]. Chinese Physics B, 2026, 35(2): 027101. doi: 10.1088/1674-1056/ae1c27

Charge-transfer-induced re-entrant ferromagnetism in twisted-bilayer-MoTe2/hBN/WSe2

  • Received Date: 17/09/2025
    Accepted Date: 29/10/2025
    Available Online: 01/02/2026
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(4)

Article Metrics

Article views(240) PDF downloads(0) Cited by(0)

Access History

Charge-transfer-induced re-entrant ferromagnetism in twisted-bilayer-MoTe2/hBN/WSe2

Abstract: Ferromagnetism in moiré flat-band systems has been extensively studied in the first valence miniband of twisted MoTe2, while its controlled realization at higher moiré fillings remains largely unexplored, except for very recent works reporting correlated magnetism near half filling of the second moiré band. Here, we investigate rhombohedral-stacked twisted MoTe2/hBN/WSe2 heterostructures and uncover two distinct ferromagnetic (FM) regions: one centered near vh ≈ 3 (half filling of the second moiré valence miniband) at zero displacement field, and a re-entrant FM phase that emerges for vh > 3 only under a finite out-of-plane electric field. These FM regions are separated by a narrow filling window with a strongly suppressed magnetic circular dichroism (MCD) response. Layer-sensitive exciton spectroscopy identifies that WSe2 is hole-doped in the re-entrant FM region, consistent with partial charge transfer from MoTe2 to WSe2. We propose that electric-field–induced layer repopulation stabilizes the re-entrant ferromagnetic phase by pinning the effective MoTe2 filling near vh ≈ 3 while adding carriers to the remote WSe2 layer. Our results demonstrate that remote-layer population control is an effective tuning knob for magnetic ordering in higher moiré minibands, extending the design space for correlated spin–valley phases in transition metal dichalcogenide heterostructures.

1.   Introduction
  • Moiré materials based on semiconducting transition metal dichalcogenides (TMDs) provide unprecedented opportunities to study quantum phases emerging from the interplay of band topology and strong correlations.[1–3] A prominent example is the realization of fractional quantum anomalous Hall (FQAH) states — fractional Chern insulators at zero magnetic field — in twisted MoTe2 (tMoTe2) and graphene-based Chern bands.[4–7] While most experimental efforts have focused on the first moiré valence flat band,[4–14] recent studies have begun to explore correlated and magnetic phenomena near half filling of the second moiré valence band in twisted MoTe2,[15–17] partly due to analogies with higher Landau levels that can host even-denominator fractional quantum Hall physics.[18–24]

    In this work, we perform magneto-optical (MCD) and exciton-sensing measurements on R-stacked tMoTe2/hBN/WSe2 devices. We detect a ferromagnetic phase centered near vh ≈ 3 (half filling of the second moiré band) at E ≈ 0, and a distinct ferromagnetic region at vh > 3 that emerges only under a finite electric field. We argue that this re-entrant high-filling ferromagnetism is consistent with an electric-field–induced charge transfer mechanism.

2.   Device structure and twist angle calibration
  • Figure 1(a) schematically illustrates the dual-gate device structure of tMoTe2/hBN/WSe2 employed in this study. Devices were fabricated using the standard tear-and-stack and dry transfer method. We use few-layer TaSe2 as contact electrodes, taking advantage of its high work function to facilitate good electrical contact for hole doping in tMoTe2. Thin flakes of hexagonal boron nitride (hBN), graphite (3–5 nm), monolayer MoTe2, monolayer WSe2, and TaSe2 (2–5 nm) were first exfoliated from bulk crystals onto Si/SiO2 (285 nm) substrates. Flakes of appropriate thickness were identified according to their reflectance contrast under an optical microscope. The MoTe2 monolayer was mechanically cut into two parts using atomic force microscope (AFM) tips. MoTe2 flakes were handled inside a liquid-nitrogen-filled glovebox with oxygen and water levels below 0.01 ppm to minimize degradation. The moiré MoTe2 bilayer and the WSe2 monolayer are separated by an ultrathin hBN layer with a thickness of approximately 1 nm. The complete dual-gated structure was assembled using a polycarbonate stamp. The stack was then released on the pre-patterned and cleaned Ti (5 nm)/Au (20 nm) electrodes on Si/SiO2 substrates, such that the graphite gates and TaSe2 grounding contact were electrically connected to the deposited contacts.

    The dual-gated structure enables independent control of the doping density (n) and the vertical electric field (E). Here, we define E = D/ε0 as the applied electric field in vacuum, where D is the displacement field and ε0 is the vacuum permittivity. The carrier density n and E on the sample are converted from the top (bottom) gate voltage Vt (Vb) using a parallel plate capacitor model

    where e is the electron charge, εb = εt = εBN is the relative dielectric constant of bottom and top hBN layers, and Ct and Cb are the top and bottom gate capacitances obtained from the top and bottom hBN thickness dt and db, which can be measured by atomic force microscopy. The offset electric field likely arises from structural asymmetry and can be determined from the symmetric axis of the dual-gate MCD map.

    Figure 1(b) illustrates the honeycomb moiré lattice with two sublattices centered at the MX and XM (M = Mo; X = Te) stacking sites. A schematic illustration of the band structures for tMoTe2/hBN/WSe2 is shown in Fig. 1(c). In the vicinity of the K point of the Brillouin zone, the band structure of each MoTe2 layer can be regarded as a single spin-polarized parabolic band. Interlayer coupling causes strong hybridization of the bands where they intersect, leading to moiré minibands. At E = 0, tMoTe2 and WSe2 have type-I band alignment with a valence band offset of ∼ 300 meV (both conduction and valence band edges originate from tMoTe2).[25] The band alignment of the sensor WSe2 and tMoTe2 valence bands ensures that the sensor remains neutral over a large range of hole doping densities. Applying an out-of-plane E-field can reduce the valence band offset, enabling conditional charge transfer.

    We first performed dielectric sensing measurements on this system. Here, monolayer WSe2 is used as a sensor. Changes in the tMoTe2 compressibility modulate the dielectric environment for the WSe2,[26] which is probed via its 2s exciton response.[27–30] The optical measurements were performed in reflection geometry using a home-built confocal optical microscope based on a closed-cycle helium cryostat equipped with a superconducting magnet. For dielectric sensing, a halogen lamp is used as a white light source. Its output is first collected by a single-mode fiber and collimated by a ×10 objective. The beam on the sample has a power below 10 nW, and the incident light is focused onto the device under normal incidence by a low-temperature microscope objective. The spot size of the excitation light is ∼ 1 μm. Reflected light is spectrally resolved by a spectrometer coupled to a liquid-nitrogen-cooled Si charge-coupled device (CCD).

    Figure 1(d) shows the 2s sensing signal of WSe2 versus vh at E = 0. Pronounced features in the resonance-energy shift are observed at vh = 1 and 2, signifying their incompressible nature (νh = 1 is defined as one hole per moiré unit cell, corresponding to a half-filled moiré valence band). No evident features of fractional fillings are observed, likely due to their much smaller gap, which is beyond the sensitivity of our measurement. In principle, n can be obtained from the capacitor model and used to calculate the twist angle from the assigned filling factors. In our case, thanks to the high mobility of the device, n (and thus the twist angle) can be independently calibrated from the quantum oscillations observed optically under an out-of-plane magnetic field of 9 T. Figure 1(e) presents the doping-dependent reflectance contrast (RC) response of WSe2 under σ+ excitation at 9 T. The oscillations result from the formation of Landau levels (LLs). Upon complete filling of the νLLth Landau level with hole carriers, the hole carrier density is expressed as nLL = νLL|B|/ϕ, where ϕ = h/e (h is Planck’s constant). The LL period is determined to be 0.160 ± 0.006 V for the Vb response, from which we deduce a hole density change of (1.36 ± 0.05) × 1012 cm−2 per volt. By determining the number of filling factors corresponding to nLL, the moiré density nM = (2.47 ± 0.07) × 1012 cm−2 is obtained. Finally, the twist angle θ is calculated to be 2.96° ± 0.04° using θ=a32nM, where a is the MoTe2 lattice constant, approximately 3.53 Å.

3.   Observation of the re-entrant FM at vh > 3
  • To investigate the filling dependence of magnetic interactions, we performed reflective magnetic circular dichroism (MCD) measurements under small B. A superluminescent light-emitting diode with a peak wavelength of 1070 nm and a full-width at half-maximum bandwidth of 90 nm was used as the light source. A combination of a linear polarizer and an achromatic quarter-wave plate generated left- and right-circularly polarized light. To avoid perturbing the system, the incident intensity on the sample was kept below 10 nW⋅μm−2. Reflected light was spectrally resolved by a spectrometer coupled to a liquid-nitrogen-cooled InGaAs one-dimensional array sensor.

    To analyze the MCD as a function of tuning parameters such as ν, E, B, and T, we integrate the MCD modulus over a spectral range that covers most of the MCD signal. The integrated MCD (referred to simply as the MCD below) reflects the difference in occupancy between the K and K′ valleys in MoTe2. Because of spin-valley locking, the signal is proportional to the out-of-plane magnetization.[31–34] In the MCD map measurements, the results are averaged over positive and negative B, i.e., MCD=MCD(+B)−MCD(−B)2.

    Figure 2(a) shows the MCD intensity plot as a function of vh and E, measured at 8 mT. MCD signals are observed at filling factors around both vh = 1 and vh = 3. In this study, we focus on the second moiré band. A clear MCD dome centered near vh = 3 appears at low |E|, signifying the emergence of magnetism around the half-filling of the second moiré band. Figure 2(b) shows the MCD versus B as a function of E at vh = 3. An appreciable hysteresis loop emerges around E = 0, confirming the ferromagnetic (FM) order. Applying a large E-field quenches the ferromagnetism around vh = 3. These observations are consistent with recent studies reporting ferromagnetism around vh = 3.[15,16]

    Strikingly, at higher fillings (vh > 3) and finite E, a second MCD-enhanced region emerges, which also exhibits magnetic hysteresis, as shown in Fig. 2(c). The re-entrant FM region shows approximately linear vh–E-field dispersion, indicating that E-field–induced charge transfer may play a role.

4.   Mechanism of the re-entrant FM
  • To uncover the origin of the re-entrant FM, we performed layer-resolved reflectance contrast (RC) measurements to identify the doping state of the WSe2 layer. Figure 3(a) shows the RC spectra as a function of Vt. We found that the neutral exciton vanishes when Vt is sufficiently negative, signifying that the WSe2 layer is hole-doped. Figure 3(b) shows the spectrally integrated RC as a function of vh and E. The bright region represents the phase space where the neutral exciton of the WSe2 layer is strong (i.e., the WSe2 layer is neutral). In contrast, the black region represents the phase space where the neutral exciton vanishes (i.e., the WSe2 layer is hole-doped). At low doping density and low E-field, the WSe2 layer is neutral, and all holes occupy the tMoTe2 layer, consistent with the type-I band alignment between tMoTe2 and WSe2. However, holes are transferred from tMoTe2 to WSe2 under a sufficiently high E-field (Ec), which decreases with increasing vh. We found that re-entrant FM appears only in the phase space where the WSe2 layer is hole-doped (Fig. 3(b)). Therefore, we propose that the re-entrant FM order observed at vh > 3 is likely induced by charge transfer between tMoTe2 and monolayer WSe2.

    Figure 3(c) schematically illustrates the band structures (hole-side only) for tMoTe2/hBN/WSe2 under zero and finite E-field. At E = 0, tMoTe2 and WSe2 have type-I band alignment with a valence band offset of ∼ 300 meV. Considering that the bandwidth and energy gap of moiré minibands are on the order of tens of meV, the Fermi level (EF) lies well above the valence band top of the WSe2 layer, and all holes reside in the tMoTe2 layer at vh≫3 without an E-field (Fig. 3(c), upper panel). Consequently, tMoTe2/hBN/WSe2 behaves similarly to bare tMoTe2, and FM order is absent until a finite E is applied. Applying an out-of-plane E-field reduces the valence band offset, moving the valence band top of the WSe2 layer closer to EF (Fig. 3(c), lower panel). Under an appropriate E-field, a certain amount of hole transfer from tMoTe2 to WSe2 occurs, keeping the effective filling factor of tMoTe2 near vh ∼ 3, resulting in re-entrant FM order in the heterostructure.

    The experimental observations are well captured by this scenario, except that the vh ∼ 3 and vh > 3 regions are separated by a magnetically suppressed corridor just above vh ≈ 3 in the MCD phase diagram. This corridor cannot be understood by classical electrostatics, in which the charge transfer should vary continuously with E and vh, and the vh ∼ 3 and vh > 3 regions should be connected. We believe this anomalous corridor is related to the strong correlation nature of the holes in tMoTe2. One possible explanation is that when vh is slightly above 3, the threshold E-field for charge transfer from tMoTe2 to WSe2 is large due to correlation effects, so the tMoTe2 bilayer becomes layer-polarized before charge transfer, resulting in vanishing FM order. In contrast, when vh is well above 3, the correlation effect is significantly suppressed by screening, resulting in a smaller E-field for charge transfer. Therefore, when charge transfer occurs, the tMoTe2 remains in a layer-hybridized state, yielding re-entrant FM order. A full microscopic validation is left for future work.

5.   Temperature dependence of the re-entrant FM
  • Finally, we study the temperature dependence of the FM order in the second moiré band. Figure 3 shows the MCD (vh, E) phase diagram at various temperatures. When the temperature is raised to 3 K, the high-filling (vh > 3) FM signal weakens markedly, while the vh ≈ 3 region remains evident, indicating a lower critical temperature for the vh > 3 region. This disparity can be understood as arising from the weakened electronic correlation and effective exchange at higher fillings in the tMoTe2 layer, due to additional screening from the excess holes transferred to the nearby WSe2 layer.

6.   Conclusion
  • In summary, we observe two distinct ferromagnetic regions in twisted MoTe2/hBN/WSe2 heterostructures: a primary dome near vh ≈ 3 at low electric field, and a re-entrant high-filling FM phase (vh > 3) that emerges only under a finite E. These regions are separated by a narrow magnetically suppressed window. Layer-sensitive exciton spectroscopy indicates that the WSe2 layer is hole-doped in the re-entrant FM region, supporting a mechanism in which electric-field–tuned layer charge transfer promotes the re-entrant FM order. These findings establish remote-layer population control as an effective approach to engineer and reconfigure correlated magnetic phases beyond the first moiré band in TMD-based systems.

Figure (4)  Reference (34)