2026 Volume 35 Issue 5
Article Contents

Yujie Wang, Xu Cheng, Jialin Shao, Xugang Qi, Jia Zhao, Lu Yang, Youwei Zhang, Bonan Zhu, Zemin Zhang. Thermally-enhanced charge collection boosts photoelectrochemical performance of hematite[J]. Chinese Physics B, 2026, 35(5): 058201. doi: 10.1088/1674-1056/ae37fc
Citation: Yujie Wang, Xu Cheng, Jialin Shao, Xugang Qi, Jia Zhao, Lu Yang, Youwei Zhang, Bonan Zhu, Zemin Zhang. Thermally-enhanced charge collection boosts photoelectrochemical performance of hematite[J]. Chinese Physics B, 2026, 35(5): 058201. doi: 10.1088/1674-1056/ae37fc

Thermally-enhanced charge collection boosts photoelectrochemical performance of hematite

  • Received Date: 02/12/2025
    Accepted Date: 08/01/2026
    Available Online: 01/05/2026
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(5)

Article Metrics

Article views(249) PDF downloads(0) Cited by(0)

Access History

Thermally-enhanced charge collection boosts photoelectrochemical performance of hematite

Abstract: The application of transition metal oxides in optoelectronics holds significant promise. However, their performance is often limited by small polaron hopping, a charge transport mechanism that reduces carrier mobility and collection efficiency. Therefore, improving small polaron hopping is crucial for enhancing charge collection. In this work, we propose a direct approach to effectively enhance the photoelectrochemical (PEC) performance of hematite by leveraging the thermal nature of polaron hopping. As a result, a photocurrent density of 4.53 mA/cm2 at 1.23 V vs. RHE was achieved by heating the photoanode to 70 °C. By combining carrier dynamics analysis with charge collection modeling, we demonstrate that heating facilitates small polaron hopping, thereby increasing carrier mobility and improving the collection efficiency of hematite photoanodes. Our work provides clear explanations of the thermal-activated small polaron hopping mechanism, offering a simple yet effective strategy for enhancing the PEC performance of transition metal oxides.

1.   Introduction
  • Photoelectrochemical (PEC) technology offers a promising route for converting solar energy directly into chemical fuels.[1,2] In a PEC device, a semiconductor photoelectrode absorbs light to generate charge carriers, which then separate and migrate to the surface to drive redox reactions.[3] Hematite (α-Fe2O3) is a particularly attractive photoanode material for this purpose due to its earth-abundant, chemical stability, and ideal band gap (2.1 eV) for visible light absorption.[4–7] However, despite these advantages, the practical application of hematite is severely limited by its intrinsically poor carrier transport properties, which lead to high rates of electron–hole recombination and consequently low energy conversion efficiency (Fig. 1(a)).[7–10]

    The root of this poor performance lies in the formation of small polarons, a process greatly facilitated by intrinsic defects within the material.[8,10,11] Under photoexcitation, electrons in α -Fe2O3 will hop from O 2p orbitals to Fe 3d orbitals (Fig. 1(bi)).[4] Instead of moving freely through the crystal lattice, photoexcited electrons localize on iron atoms, creating a localized lattice distortion, known as a small polaron. This intense localization creates a strong electrostatic interaction that physically distorts the surrounding lattice.[4,12] Charge transport then occurs via a slow, thermally-activated “hopping” of these polarons between lattice sites, rather than through fast band-like conduction (Fig. 1(bii)).[13–15] Oxygen vacancies (OV) are intrinsic defects in α-Fe2O3, and act as trapping sites that further localize polarons and exacerbate recombination.[16,17]

    To address this critical transport limitation, research has primarily focused on strategies like elemental doping and surface passivation. Doping can modify the electronic environment to lower the energy barrier for polaron hopping, while surface passivation aims to reduce the density of surface defects (including OV).[18–20] While effective to some extent, these methods often involve complex, multi-step fabrication processes that may introduce impurities or create secondary issues. We propose a more direct approach: leveraging the thermal nature of polaron hopping.[10,14,21,22] Since hopping is a thermally-activated process, raising the temperature can increase the hopping frequency and liberate polarons from trapping sites, effectively increasing charge carrier mobility (Fig. 1(biii)).[10,11,21,23]

    In this work, we thoroughly investigated the thermally-regulated dynamics of small polarons in α-Fe2O3 combining computational and experimental approaches. Annealing α-Fe2O3 samples in an argon atmosphere increases the concentration of OV, giving rise to defect states within the band gap as indicated by density functional theory (DFT) calculations. This increases the probability of small polaron formation, facilitating our study of small polarons within the samples. Calculations of carrier separation and injection efficiency, as well as mobility tests, demonstrate that temperature elevation promotes small polaron hopping and increases the carrier mobility, which is the primary reason for the enhanced PEC performance. Ultimately, analysis of the spatial loss rate (SLR) suggests that elevated temperature enhances the carrier collection efficiency. Our work provides a practical and effective approach for enhancing the water-splitting performance of small polaron dominated transition metal oxides.

2.   Results and discussion
  • Figure 2(a) depicts a cross-section scanning electron microscope (SEM) of α-Fe2O3, with an approximate thickness of 200 nm. The plane-view SEM and energy dispersive spectrometer (EDS) are available in Figs. S1 and S2.[24] X-ray diffraction (XRD) was performed on the film after being annealed at 700 °C in an argon atmosphere on an FTO substrate. The resulting pattern demonstrates that the α-Fe2O3 is well-oriented on the (110) crystal plane (Fig. 2(d)).[25] XRD patterns of other treated hematite samples are presented in Fig. S3. To probe the effect of the annealing atmosphere, x-ray photoelectron spectroscopy (XPS) was used. The spectra for the O 1s orbitals (Figs. 2(b) and 2(c)) indicate that the argon annealing process yields a higher concentration of OV compared to annealing in air.[8,26,27] DFT calculations were performed to understand the electronic impact of these vacancies. The calculated density of states (DOS) and energy band structures (Fig. S4) show that introducing OV creates a new defect state at the bottom of the conduction band (Fig. 2(f)), which is absent in the defect-free α-Fe2O3 (Fig. 2(e)). Such a defect state, positioned within the band gap or slightly below the CBM, serves as an electron trapping site, leading to significant charge localization and concomitant local lattice distortions, key hallmarks of small polaron formation.[15,28] This phenomenon is critical for understanding charge transport and photocatalytic activity in α-Fe2O3. Therefore, to study this phenomenon in depth, the argon-treated α-Fe2O3 samples with higher vacancy concentration were selected for all subsequent experiments.

    Figure 2(g) illustrates in-situ Raman spectra of the α-Fe2O3, recorded using 633 nm optical excitation at temperatures ranging from room temperature down to −180 °C. It can be observed that the intensity of each peak decreases in proportion to the increase in temperature, and the Raman peaks are red-shifted.[29,30] This is because higher temperatures enhance phonon–phonon interactions and anharmonic electron–phonon coupling.[30–32] These intensified interactions weaken the strong coupling between electrons and specific phonon modes, thereby reducing the localization of small polarons. This, in turn, strengthens lattice vibrations, causing the red shift of the Raman peaks.[30–32] Simultaneously, the lattice undergoes thermal expansion, leading to a shallower depth of the localized lattice distortion potential well and lowering the energy barrier for confining small polarons. Meanwhile, the lattice thermal expansion also weakens thermal conductivity and reduces the Raman peak intensity.[30,32] These synergistic effects collectively lower the activation energy required for small polarons hopping, enhancing the charge transport capabilities. The Raman spectrum taken at room temperature with 532 nm photoexcitation is provided in Fig. S5.

  • The PEC characteristics of the argon-treated α-Fe2O3 photoelectrodes were investigated, focusing on the effects of operating temperature. Linear scan voltammetry (LSV) under simulated AM 1.5G solar illumination shows that heating the system significantly boosts performance (Fig. 3(a)). Figure S6 shows that introducing OV results in a greater increase in performance after heating. At a potential of 1.23 V vs. RHE, the net photocurrent density increased by a factor of 1.69, rising from 2.68 mA/cm2 at 25 °C to 4.53 mA/cm2 at 70 °C. This enhancement is supported by incident photon-to-current conversion efficiency (IPCE) measurements (Fig. 3(b)), which show a 1.6-fold increase at a wavelength of 360 nm at 70 °C compared to room temperature. These results clearly demonstrate that heating is a simple and effective technique for improving the photoelectrode’s performance.

    To determine the cause of this improvement, the physical properties of the α-Fe2O3 film were analyzed. The light absorption increased only marginally upon heating and is thus an unlikely contributor to the large performance gain (Fig. S7). Similarly, Mott–Schottky analysis (Fig. 3(c)) revealed that the carrier concentration rose only slightly, from 5.2 × 1019 cm−3 at 25 °C to 7.1 × 1019 cm−3 at 70 °C (the detailed calculation procedure is described in Eq. (S1)). In contrast, electrochemical impedance spectroscopy (EIS) showed a notable reduction in the impedance arc radius upon heating, which corresponds to a lower charge transfer resistance and more efficient charge transfer at the electrode–electrolyte interface (Fig. 3(d)).[9,10,20,23]Figure S8 presents the significantly increased absorbed photon to current conversion efficiency (APCE) of α-Fe2O3 at elevated temperatures, corresponding to the improved charge collection, as calculated in detail in Eq. (S2).

    The most critical factor was identified by analyzing the transfer curves (Figs. 3(e) and 3(f)). From this, the carrier mobility increased dramatically by approximately 6.5 times, from 2.99 × 10−3 cm2/(V·s) at 25 °C to 1.943 × 10−2 cm2/(V·s) at 70 °C, as calculated in Eq. (S3).[33] Therefore, we conclude that the improved PEC performance is primarily driven by the thermally-enhanced carrier mobility. This facilitates the hopping of small polarons within the bulk α-Fe2O3, leading to superior charge separation and transfer efficiency.

    Additionally, the α-Fe2O3 film demonstrates promising operational stability. Chronopotentiometry (CP) testing at 70 °C (Fig. S9(a)) reveals an initial gradual increase in current, followed by stabilization and a slight decrease. The transient current spike observed around 32000 s is likely attributable to the detachment of bubbles from the electrode surface. Post-test characterization confirms the structural and chemical integrity of the film. The O 1s XPS spectra (Fig. S9(d)) remain virtually unchanged, showing no indication of excessive oxygen vacancy formation. XRD patterns (Figs. S9(b) and S9(e)) exhibit no peak shifts or new phases, ruling out any phase transformation. Furthermore, SEM images (Figs. S9(c) and S9(f)) confirm that the film remains adherent and intact, with no signs of delamination or morphological degradation. Collectively, these results confirm that the α-Fe2O3 film retains its original morphology, crystal structure, and surface chemistry after 12 h of continuous operation at elevated temperature, underscoring its robust stability.

  • Elevating the temperature of α-Fe2O3 samples promotes the small polaron hopping, which in turn improves the charge separation and injection efficiency.[10,23] To confirm this, we measured these efficiencies under simulated solar irradiation. Furthermore, the role of small polarons in different hopping modes was tested under 360 nm and 525 nm monochromatic light, corresponding to ligand-to-metal charge transfer (LMCT) and d–d transitions, respectively.[34,35] Calculations of the theoretical maximum photocurrent densities for three wavelengths and the charge separation and injection efficiency are given in Eqs. (S4)–(S6).

    Figure 4(a) shows the charge injection (ηinj) and separation (ηsep) efficiencies of α-Fe2O3 under simulated solar light. While heating improves both, the enhancement in ηsep is more pronounced. These values were calculated by the following equations:

    where Δηinj and Δηsep represent the percentage increases in charge injection and separation efficiencies, while αinj and αsep represent the percentage increases in charge injection and separation efficiencies as percentages of the total increase. As detailed in Fig. 4(b), which quantifies these percentage increases at different potentials, the photocurrent gain is primarily due to improved charge separation. This confirms that heating’s main effect is to facilitate small polaron hopping.

    This mechanism is consistent under monochromatic light. Figs. 4(c) and 4(e) present ηinj and ηsep under 360 nm and 525 nm light, respectively, with their contributions to photocurrent shown in Figs. 4(d) and 4(f). Under 360 nm light, which excites carriers via LMCT, the absolute ηsep is higher.[34] LMCT, in Fig. 4(h), involving electron excitation from O 2p to Fe 3d orbitals, directly generates mobile carriers that contribute to photocurrent.[34,36] Under 525 nm light, which induces a d–d transition, the percentage increase in ηsep upon heating is greater (Fig. 4(g)).[34] The d–d transition is more localized (Fig. 4(i)), creates more small polarons, and does not directly produce mobile carriers.[7,36,37] Consequently, heating has a more significant relative effect by promoting small polaron hopping in this regime.

    To further validate this, we compared α-Fe2O3 samples annealed in argon (creating more OV and small polarons) with those annealed in air under solar light (Fig. S10). As expected, the argon-annealed samples showed a significantly larger increase in separation efficiency and photocurrent density after heating. This directly demonstrates that enhancing small polaron hopping is crucial for improving PEC performance.

  • To evaluate carrier collection and loss during photoelectrode operation intuitively, we employ an optical model based on the transfer matrix method (TMM).[9,38,39] Accurate measurement of the optical constants of thin films is a prerequisite for the construction of the transport matrix model. In this work, a multi-angle elliptical polarimeter combined with parameter fitting was used to extract the optical constants of α-Fe2O3 thin film, and detailed optical constants n and k are provided in Fig. S11. The detailed calculation process is provided in Eqs. (S7)–(S11). Figure 5(a) depicts a schematic of the model’s structure, assuming that the α-Fe2O3 photoelectrode anode is one-dimensional and has a completely flat surface. As can be seen, the incident light must pass through numerous layers of media, and phase cancellation is utilized to deal with repeated reflections from incoherent layers. The film’s optical constants were eventually employed to calculate the position-dependent photogenerated carrier generation profile within the active layer, as illustrated in Fig. 5(b). The results reveal that the carrier generation rate G(Z) decreases dramatically from surface to film. As previously stated, the regularization procedure generates SLR curve for each IPCE spectrum, which reflects the system’s carrier collection characteristics.[7,9,38,39] Figure 5(c) depicts the SLR curve obtained from Fig. 3(b), revealing that the majority of the collected carriers are created within the first 100 nm of the electrode surface. Figure 5(c) shows that the SLR of α-Fe2O3 at 70 °C is much lower than that at 25 °C, accounting for approximately 40% of 25 °C at the surface. In the PEC system, the material performance is determined by the minority carrier collection length, Lc, which reflects the distance at which the minority carriers effectively affect the surface current.[8,38] By defining Lc as the distance from the position where the carrier collection efficiency is 1/10 of the surface carrier collection efficiency to the surface, Fig. 5(d) shows that the Lc of α-Fe2O3 at 70 °C is 8 nm longer than at 25 °C, implying that increasing the temperature promotes the hopping of the small polarons, resulting in a significant increase in the carrier collection efficiency.[9]

3.   Conclusions
  • In summary, we report a thermal activation strategy that dramatically improves the performance of hematite photoanodes by enhancing small polaron hopping, which is the main charge transport mechanism in many transition metal oxides. Unlike conventional doping or passivation, this method uses elevated temperature to directly facilitate polaron hopping, increasing carrier mobility by ∼ 6.5 times and reducing spatial losses. The thermal effect is most pronounced for charges excited via d–d transitions due to their strong polaronic nature. Consequently, the optimized device achieves a high photocurrent density of 4.53 mA/cm2 at 1.23 V vs. RHE. This work establishes a simple and widely applicable approach to achieve efficient carrier transport in metal oxide photoelectrodes for solar energy conversion.

Figure (5)  Reference (39)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return