2026 Volume 35 Issue 5
Article Contents

Yi-Ran Li, Yong-Hao Gao, Xiao-Qin Lu, Ping Su, Hui Liang, Ying Zhou, Dan-Dan Wu, Yan Sun, Qiu-Ju Li, Jin-Yu Liu, Shou-Guo Wang, Gang Chen, Tian-Long Xia, Na Li, Xue-Feng Sun, Yi-Yan Wang. Power-law scaling of low-temperature effective mass in La3ScBi5[J]. Chinese Physics B, 2026, 35(5): 057107. doi: 10.1088/1674-1056/ae39d1
Citation: Yi-Ran Li, Yong-Hao Gao, Xiao-Qin Lu, Ping Su, Hui Liang, Ying Zhou, Dan-Dan Wu, Yan Sun, Qiu-Ju Li, Jin-Yu Liu, Shou-Guo Wang, Gang Chen, Tian-Long Xia, Na Li, Xue-Feng Sun, Yi-Yan Wang. Power-law scaling of low-temperature effective mass in La3ScBi5[J]. Chinese Physics B, 2026, 35(5): 057107. doi: 10.1088/1674-1056/ae39d1

Power-law scaling of low-temperature effective mass in La3ScBi5

  • Received Date: 10/11/2025
    Accepted Date: 17/01/2026
    Available Online: 01/05/2026
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(5)

Article Metrics

Article views(177) PDF downloads(1) Cited by(0)

Access History

Power-law scaling of low-temperature effective mass in La3ScBi5

Abstract: The variation of the effective mass m* of carrier is often overlooked in experimental studies on quantum oscillations and Kohler’s rule. Here, we report the magnetotransport properties of La3ScBi5 and reveal the changing m* in it. The temperature and magnetic field dependence of m* follows the power-law scaling behavior at low temperature and leads to the failure of conventional analysis, which should not be ignored. In the analysis of the thermal factor and Dingle plot of de Haas–van Alphen oscillation in La3ScBi5, satisfactory fitting results can be obtained after considering the correction of m*. We have also applied this method to Sr1−yMn1−zSb2, solving the remaining fitting problem in previous reports. Moreover, the magnetoresistance (MR) of La3ScBi5 has been found to violate Kohler’s rule. Although the extended Kohler’s rule is applicable to high-temperature MR data, it does not scale the low-temperature data well. We further modified the extended Kohler’s rule by introducing m*, and subsequently scaled the low-temperature MR data well. Our study emphasizes the importance of considering the variation of m* in the analysis of quantum oscillations and Kohler’s rule, and provides a method for extracting the temperature and magnetic field dependence of m* through quantum oscillations, which is very beneficial for the data analysis of other materials in the future.

1.   Introduction
  • Quantum oscillation has been a powerful experimental technique for exploring the underlying physics in materials. Quantum oscillations mainly include the de Haas–van Alphen (dHvA) oscillation in magnetization and the Shubnikov–de Haas oscillation in resistivity. Recently, Wang et al. discovered a new type of quantum oscillation with the logB periodicity in ZrTe5.[1] Chen et al. observed the oscillation of resistivity and specific heat with temperature under a constant magnetic field in NdAlSi.[2] The Lifshitz–Kosevich (LK) theory is commonly used to describe the quantum oscillations.[3] By analyzing the quantum oscillations using the LK formula, some parameters can be obtained, such as the effective mass m*, Dingle temperature, and Berry phase.

    Kohler’s rule is an important law related to the magnetoresistance (MR) of materials, which states that the MR should be a function of B/ρ0 and follow the scaling behavior MR = f(B/ρ0) (ρ0 is the resistivity at zero field).[4] Luo et al. pointed out that the more exact form of Kohler’s rule is MR = f(Bτ) with τ being the relaxation time of carriers.[5] Recently, Xu et al. proposed the extended Kohler’s rule MR = f(B/nTρ0), where nT describes the relative change in the carrier concentration induced by thermal excitation.[6] The extended Kohler’s rule can effectively explain the violation of Kohler’s rule in some materials,[6–8] such as TaP, InSb, TaCo2Te2, and HfSe1.9.

    However, whether in the analysis of quantum oscillations or Kohler’s rule, m* is always treated as an invariant constant. In this paper, we have studied the dHvA oscillations and Kohler’s rule in La3ScBi5 and found that the temperature and magnetic field dependence of m* should not be ignored. m* follows the power-law scaling behavior at low temperature due to the effective mass renormalization by the long-range Coulomb interaction. The conventional analysis based on the LK formula fails to fit the oscillation data of La3ScBi5. The better fits are obtained after considering the correction of m*, indicating that m* in La3ScBi5 changes with temperature and magnetic field. In addition, the MR has been found to violate Kohler’s rule, and even the use of extended Kohler’s rule is not enough for scaling the low-temperature data. By introducing the magnetic field and temperature dependence of m* obtained from the quantum oscillation, the extended Kohler’s rule is further modified to MR = f(Bm*/nTρ0), which can effectively scale the low-temperature MR data.

2.   Results and discussion
  • La3ScBi5 is a member of the Ln3MPn5 (Ln = lanthanide; M = metal; Pn = pnictide) family,[9–17] and its crystal structure contains 1D Bi chain and a distorted kagome lattice.[18] The band structure calculations reveal that multiple types of Dirac fermions coexist in La3ScBi5, including type-I, type-II, higher-order quadratic and nodal-line.[18]

    Figures 1(a)–1(c) plot the isothermal magnetization of La3ScBi5 as a function of magnetic field in the directions of B ⊥ bc, B ∥ b and B ∥ c, respectively. Strong dHvA quantum oscillations can be observed in these three directions under low temperature and strong magnetic field. For the directions within the distorted kagome lattice plane (B ⊥ bc and B ∥ b), there are small kinks induced by the Zeeman effect in high fields [red arrows in Figs. 1(a) and 1(b)], similar to those in ZrGeSe[19] and Sn4P3.[20] In low fields, it seems to have a very low-frequency oscillation. This possible low-frequency oscillation has little impact on high magnetic field amplitude, but it will affect the background extraction of high-frequency oscillations. For the accuracy of the analysis of high field oscillation, such a low-frequency oscillation is ignored when extracting the background. The insets of Figs. 1(d)–1(f) show the oscillatory components of magnetization (ΔM = M – 〈M〉) after subtracting the smooth background 〈M〉. The corresponding fast Fourier transformation (FFT) spectra are displayed in the main images of Figs. 1(d)–1(f).

    The anisotropy of magnetization in La3ScBi5 is interesting. The magnetization is dominated by paramagnetism in the B ⊥ bc and B ∥ b directions, but exhibits diamagnetism in the long-axis direction (B ∥ c). This situation is different from the unusual axial diamagnetism in La3MgBi5, where the magnetization is dominated by diamagnetism in the directions of the crystal axis (B ∥ a, b, c).[11] The axial diamagnetism in La3MgBi5 originates from the restricted motion of the Dirac fermion at the Fermi level. The anisotropic magnetization in La3ScBi5 can be attributed to the type-I Dirac fermion located near the Fermi level in the Γ–A direction.

    The dHvA quantum oscillation can be described by the LK formula[3,21–23]

    In the formula, RT and RD represent the variation of oscillation amplitude with temperature and magnetic field, respectively. m* is the cyclotron effective mass of carrier. TD is the Dingle temperature. 2πβ is the Berry phase and δ is a phase shift. The thermal factor RT is often used to fit the temperature dependence of FFT amplitude and extract the effective mass m*. The main image in Fig. 2(a) shows the RT fittings of frequency F1 in the B ⊥ bc direction. The black solid line is the fit made by including all obtained data points. Clearly, conventional thermal factor RT cannot describe the data well. A better fit can be obtained if the data points below 5 K are not included [red solid line in Fig. 2(a)]. Here, we propose that the failure of conventional RT fitting can be attributed to changes in the effective mass m* of carrier. In previous studies on quantum oscillations, m* was always treated as a constant. However, in reality, m* can vary with temperature.[6,24] By considering the influence of the long-range Coulomb interaction,[18,25] the dependence of m* on temperature can be taken as m* ∝ (T + T0)m1, and then the temperature term in RT becomes T(T + T0)m1 (m1 = 0 corresponds to the conventional RT). As shown in Fig. 2(d), the data can be well fitted using this modified RT, and the goodness-of-fit has increased from 0.9807 (F1) / 0.9743 (F2) to 0.9951 (F1) / 0.9949 (F2). For frequencies F1 and F2 in the B ⊥ bc direction, the m* terms obtained by fitting are (T + 0.60)−0.36 and (T + 1.83)−0.45, respectively. The frequency in the B ∥ b direction exhibits a similar phenomenon [Figs. 2(b) and 2(e)]. The modified RT fitting improved the goodness-of-fit from 0.9916 to 0.9997 and generated a m* term (T + 2.83)−0.37. The situation is different in the B ∥ c direction, and using conventional RT to fit can produce acceptable results [Fig. 2(c)], which means that the temperature dependence of m* in this direction is relatively weak. However, it should be noted that using the modified RT can achieve better fittings [Fig. 2(f)]. The obtained m* terms for frequencies F1 and F2 in the B ∥ c direction are (T + 1.97)−0.20 and (T + 2.87)−0.20, respectively.

    By comparing the fitting results of the three directions in Fig. 2, three main conclusions can be drawn. (i) The temperature dependence of m* has a significant impact on the amplitude of quantum oscillations. The stronger the temperature dependence of m* (m1 deviates from 0), the worse the description of oscillation amplitude by conventional RT. (ii) The modified RT can fit the data well and extract the temperature dependent behavior of m*. (iii) The temperature dependence of m* in La3ScBi5 exhibits obvious anisotropy, which is stronger in the distorted kagome lattice plane but weaker in the long-axis direction. In La3ScBi5, the effective mass follows the power-law scaling behavior m* ∝ (T + T0)m1 at low temperature. In fact, such a temperature dependent behavior of m* has been theoretically obtained in three-dimensional systems with long-range Coulomb interaction.[25] The numerical calculation results show that the temperature dependence of m* is only significant under long-range Coulomb interaction, indicating a close relationship between them.[25] Similar power-law scaling behavior of m* also appears in some strongly correlated systems, such as heavy fermions,[26] which is not the case in La3ScBi5. The electron–phonon interaction is also not expected to dominate the correction of m*, as m* follows the power-law scaling behavior and increases with decreasing temperature, but the phonon occupation number decreases at low temperatures. The above results not only indicate the validity of the modified RT, but also suggest that the long-range Coulomb interaction plays an important role in La3ScBi5 and causes the changes of m*. Especially, this method is universal and can also be applied to other materials, such as an established magnetic topological semimetal Sr1−yMn1−zSb2.[18,22]

    Since m* can vary with temperature, it is natural to wonder if m* will vary with a magnetic field. This question can be explored by studying the Dingle plot. According to the LK formula, if ln[D] [D=ΔMBsinh(λT)] is plotted as a function of 1/B, the image will be a linear line with a fixed slope. Such a Dingle plot is often used to extract Dingle temperature TD from the fitted slope. However, the premise of the above operation is that m* does not change with B. Figures 3(a) and 3(b) show the conventional Dingle plots of F1 in the B ⊥ bc and B ∥ b directions, respectively. Clearly, the data points do not present a straight line, indicating a nonlinear relationship between ln[D] and 1/B. Similar to the temperature dependence of m*, taking m* ∝ (B + B0)m2, the magnetic field term in RD will become (B + B0)m2/B (m2 = 0 corresponds to the conventional RD). As shown by the red solid lines in Figs. 3(a) and 3(b), the data can be well fitted after considering the magnetic field dependence of m*. The obtained m* terms are (B + 0.63)−3.79 and (B + 0.25)−1.48, respectively. Furthermore, the Dingle plot can be modified using fitted values of m2 and B0. If the power exponent of B in the horizontal and vertical axes is corrected to (B + B0)m2/B, the data points will fall on a straight line [Figs. 3(c) and 3(d)], which returns to the linear description of the conventional Dingle plot. Therefore, in La3ScBi5, the magnetic field will have a significant impact on m*. The magnetic field dependent m* may be another characteristic of long-range Coulomb interaction systems, which requires further theoretical research.

    After characterizing the magnetic properties, the electrical transport properties of La3ScBi5 have also been investigated. As shown in the inset of Fig. 4(a), the resistivity of La3ScBi5 exhibits the metallization behavior. Figures 4(a) and 4(b) show the MR in the range of 1.8 K–25 K and 30 K–300 K, respectively. The curvature of the MR curves varies at different temperatures. The curves are concave at temperatures above 30 K. However, the curves become convex at temperatures below 25 K, which is the result of the weak antilocalization effect.[27,28] The MR data for the entire temperature range can be well fitted using the typical power law MR ∝ Bt. The obtained values of t are presented in the inset of Fig. 4(b). The variation of t can also clearly reflect the concavity and convexity of the curves.

    Figure 4(c) shows the MR of La3ScBi5 plotted against B/ρ0. Clearly, the MR curves at different temperatures do not collapse onto a single curve, indicating the violation of Kohler’s rule MR = f(B/ρ0). The violation of Kohler’s rule in La3ScBi5 is not expected, as the Hall resistivity exhibits a single band behavior.[18] In order to further understand the MR behavior, the extended Kohler’s rule MR = f(B/nTρ0) has been employed to scale the MR data. As shown in Fig. 4(d), the curves can roughly collapse onto a single curve. Although the extended Kohler’s rule can effectively scale the MR data above 30 K, it is not ideal for data below 30 K. There are two interesting phenomena that need to be noted here. Firstly, the carrier concentration of La3ScBi5 is high.[18] The violation of Kohler’s rule is more commonly observed in topological semimetals or semiconductors, as their low carrier concentration makes the thermal factor nT more sensitive to temperature.[6] For typical metals with high carrier concentration, nT becomes less sensitive to the change of temperature. However, La3ScBi5 has a high carrier concentration and exhibits a clear violation of Kohler’s rule. This may indicate that the Dirac fermions near the Fermi level dominate electrical transport in La3ScBi5. Secondly, the curves in Fig. 4(d) only roughly collapse onto one curve but do not completely overlap, which means that even the extended Kohler’s rule cannot perfectly describe the case in La3ScBi5.

    In fact, a modified scaling form MR = f(Bτ) has been introduced in a previous study,[5] where τ is the relaxation time of carriers. Bτ can be represented as Bτ = (m*/e2)B/(nρ0) by using ρ0 = m*/(ne2τ). Therefore, the scaling behavior MR = f(B/nTρ0) of the extended Kohler’s rule will be obtained if m* is temperature independent.[6] Even if m* is not temperature independent, the extended Kohler’s rule is still valid because the influence of temperature on m* can be included in nT. However, the magnetic field dependence of m* has been ignored in the above analysis. By introducing the temperature and magnetic field dependence of m*, the extended Kohler’s rule can be further modified to MR = f(Bm*/nTρ0). As shown in Fig. 5, after considering the variation of m*, the MR curves at low temperature are well scaled onto a single curve, indicating that the failure of the extended Kohler’s rule at low temperature comes from the change of m* with magnetic field. The introduction of m* will lead to the change of curve behavior. Unlike the Kohler’s rule or the extended Kohler’s rule, here the x-axis variable has changed from B to B(B + B0)m2. In the current analysis of La3ScBi5, as the magnetic field increases, the value of B(B + B0)m2 will first increase and then decrease, resulting in the curve behavior shown in Fig. 5. However, no matter how the curve behavior changes, the MR curves at low temperature can still be well scaled to the same curve, indicating the effectiveness of the modification of the extended Kohler’s rule by m*.

3.   Summary
  • In summary, we have grown high-quality single crystals of La3ScBi5, which exhibit strong dHvA quantum oscillations. In the process of analyzing quantum oscillations, it was found that m* changes with temperature and magnetic field rather than remaining a constant, leading to the failure of conventional fits. The better fits have been obtained through the correction of m*. The MR of La3ScBi5 exhibits a violation of Kohler’s rule. Even the extended Kohler’s rule is only applicable to scaling the high-temperature data. The extended Kohler’s rule is further modified by considering the variability of m*, after which the MR at low temperature can be well scaled.

Figure (5)  Reference (28)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return