2026 Volume 35 Issue 8
Article Contents

Qinghui Yu, Xue He, Yongli Yu, Xiuqiao Liu, Shilei Ding, Rui Wu. Cubic magnetocrystalline anisotropy-driven spin reorientation in TmIG detected by spin Hall magnetoresistance[J]. Chinese Physics B, 2026, 35(8): 087202. doi: 10.1088/1674-1056/ae5a14
Citation: Qinghui Yu, Xue He, Yongli Yu, Xiuqiao Liu, Shilei Ding, Rui Wu. Cubic magnetocrystalline anisotropy-driven spin reorientation in TmIG detected by spin Hall magnetoresistance[J]. Chinese Physics B, 2026, 35(8): 087202. doi: 10.1088/1674-1056/ae5a14

Cubic magnetocrystalline anisotropy-driven spin reorientation in TmIG detected by spin Hall magnetoresistance

  • Received Date: 06/03/2026
    Accepted Date: 31/03/2026
    Available Online: 01/08/2026
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Figures(4)

Article Metrics

Article views(54) PDF downloads(1) Cited by(0)

Access History

Cubic magnetocrystalline anisotropy-driven spin reorientation in TmIG detected by spin Hall magnetoresistance

Abstract: The precise manipulation and detection of magnetization in magnetic insulators are essential for the development of next-generation spintronic devices. Here, using a heterostructure consisting of a heavy metal and a magnetic garnet thin film, i.e., (111)-oriented Pt/Tm3Fe5O12 (TmIG), we reconstruct the three-dimensional magnetization reversal trajectory using spin Hall magnetoresistance (SMR). It is found that the SMR signal of the heterostructure exhibits abrupt jumps when the magnetic field is scanned along the out-of-plane direction, and this anomalous phenomenon persists at temperatures below 100 K. By employing a three-dimensional Stoner–Wohlfarth model, we demonstrate that this behavior originates from a discontinuous magnetization trajectory with a unique 3m symmetry, which is governed by the competition among the cubic magnetocrystalline anisotropy, magnetoelastic anisotropy, and the Zeeman energy. These results provide a novel strategy for detecting three-dimensional magnetization orientation in magnetic insulators and hold the potential to advance the development of low-energy-consumption spintronic devices.

1.   Introduction
  • The electrical manipulation and detection of magnetic order in heavy metal (HM)/magnetic insulator (MI) heterostructures are central to the advancement of low-power spintronic devices.[1,2] In these systems, the interaction between interfacial magnetization and spin currents gives rise to spin Hall magnetoresistance (SMR), enabling the sensitive electrical readout of the magnetization orientation in the adjacent MI layer.[3–5] As a result, SMR has been widely employed to investigate HM/MI systems,[6–11] with a particular focus on HM/yttrium iron garnet (Y3Fe5O12, YIG)[12–14] and other rare-earth iron garnets (REIG), formed by substituting Y with rare-earth elements,[8,15–18] mainly due to their high Curie temperature, low damping constant, and long spin transport distance.[19–21]

    Compared to YIG, Tm3Fe5O12 (TmIG) exhibits significant magnetic anisotropy, especially magnetoelastic anisotropy, which is considered to be the origin of robust perpendicular magnetic anisotropy (PMA) in TmIG thin films.[22,23] However, the magnetocrystalline anisotropy (MCA) in TmIG thin films has often been considered secondary to magnetoelastic anisotropy,[23,24] and has therefore frequently been neglected due to its relatively small magnitude.

    Recently, field-free spin–orbit torque (SOT) switching of magnetization has been achieved by exploiting the intrinsic cubic MCA in (111)-oriented TmIG films with PMA,[25,26] indicating the non-negligible contribution of cubic MCA to the magnetization switching process. This field-free SOT switching arises specifically in (111)-oriented thin films, where the projection of MCA onto the (111) plane exhibits spontaneous mirror-symmetry breaking.[25] This symmetry breaking acts as an azimuth-dependent effective field that theoretically couples the perpendicular reversal with complex in-plane dynamics. However, anomalous Hall effect (AHE) measurements can only probe the out-of-plane component of the magnetization and therefore cannot fully resolve the three-dimensional magnetization state.[5] Thus, reliable detection and reconstruction of three-dimensional magnetization reversal, including both out-of-plane and in-plane magnetization components in REIG thin films, are still lacking. In contrast, SMR enables the reconstruction of three-dimensional magnetization trajectories under a perpendicular magnetic field, thereby allowing direct mapping of the magnetization switching path.

    In this work, we investigate the magnetic field dependence of SMR in the Pt/(111)-TmIG heterostructure with easy-plane magnetic anisotropy, which is beneficial for continuously tracking the in-plane magnetization during a relatively slow reversal process. The SMR, which is sensitive to the in-plane magnetization, is employed to detect the three-dimensional magnetization reversal. Our transport measurements reveal that the SMR curves exhibit hysteresis and sharp jumps between high- and low-resistance states below 100 K, resembling the tunneling magnetoresistance (TMR) behavior in traditional magnetic tunnel junctions. By employing a three-dimensional Stoner–Wohlfarth (S–W) model, we demonstrate that the out-of-plane mirror-symmetry breaking associated with cubic MCA, together with field-induced in-plane rotation-symmetry breaking, collectively drives spin reorientation, giving rise to the anomalous sharp jumps observed in the SMR. These results clarify the role of cubic MCA in magnetization reorientation within REIG heterostructures.

2.   Experimental details
  • The high-quality single-crystal TmIG thin film was grown on the (111)-oriented GGG substrate by pulsed laser deposition (PLD) using a KrF excimer laser (λ = 248 nm) from a stoichiometric TmIG target. The film was deposited at a substrate temperature of 670 °C and a laser fluence of 2 J⋅cm−2. To obtain in-plane magnetic anisotropy (IMA) TmIG films, an oxygen pressure of 15 Pa was adopted, which is lower than the optimal pressure for PMA.[27] After deposition, the film was cooled down to room temperature at a rate of 10 °C/min while maintaining the oxygen pressure. The surface morphology was characterized using an atomic force microscope (AFM) (Bruker, ICON). The magnetic properties and electrical transport properties were measured using a physical properties measurement system (Quantum Design, PPMS Dynacool). For the transport measurements, a 4-nm-thick Pt layer was deposited on the TmIG film in an ultra-high-vacuum magnetron sputtering chamber, and the resulting Pt/TmIG heterostructure was then patterned into 10 μm × 15 μm Hall bars via photolithography. The current channel of the Hall bars was aligned with the [112¯] direction of the thin film.

3.   Results and discussion
  • The AFM image of the TmIG film reveals an atomically flat surface with a root-mean-square (RMS) roughness of about 0.12 nm (Fig. 1(a)). The in-plane magnetic hysteresis shows a square loop with a high remanence ratio, indicating strong IMA in this sample from 10 K to 300 K (see supplementary materials Section 1). Figure 1(b) shows the representative in-plane (IP) hysteresis loop measured at 80 K, which exhibits a saturation magnetization (Ms) of 96 kA/m. Notably, no magnetic compensation was observed across the entire temperature range (see supplementary Fig. S1), consistent with previous reports.[5,23,28]

    The measurement schematic is shown in Fig. 1(c), and Fig. 1(d) illustrates the field dependence of the transverse SMR RT measured at 80 K with a magnetic field applied along the out-of-plane (OOP) direction. The applied current density is fixed at 2 × 106 A⋅cm−2. The measured RT shows an anomalous feature that deviates from conventional SMR behavior. Specifically, the curve exhibits a step-like hysteresis loop characterized by sharp transitions between high- and low-resistance states, which resemble the typical characteristics of TMR.[29,30] However, the TMR mechanism can be excluded since our device contains only a single ferromagnetic layer. Furthermore, such step-like features appear in both the transverse and longitudinal channels of the Hall bar. Therefore, we attribute this feature to the abrupt in-plane magnetization reorientation during the reversal process, because both transverse and longitudinal SMR are sensitive to the in-plane components of the magnetization.

    To elucidate the anomalous field dependence of SMR, we perform numerical simulations using the three-dimensional S–W model[31] under the coherent rotation assumption. The total energy is given by:[23,25]

    where θM and φM are the polar and azimuthal angles of the magnetization with respect to the [111] and [112¯] axes, respectively. The parameters Kc1,2 and Ku1,2 denote the first- and second-order constants of the cubic MCA and uniaxial magnetoelastic anisotropy, respectively; Ms, H, and δ represent the saturation magnetization, the magnitude of the external field, and the angle between the magnetization and the external field, respectively. It should be noted that a coordinate transformation was performed on the classical cubic MCA formula to unify the angular definitions, yielding the transformed direction cosine polynomials Kc1F1(θM, φM) and Kc2F2(θM, φM) (the detailed derivation is provided in supplementary materials Section 2; supplementary Fig. S2 shows the energy landscape of the cubic MCA before and after the coordinate transformation).

    Powell’s algorithm[32] was used to determine the energy-minimizing equilibrium state (θM, φM) for each external field H, and the transverse and longitudinal SMR curves were then calculated using:[5,8,12,33]

    where θ and φ denote the polar and azimuthal angles of the magnetization with respect to the film normal and the current direction (θ = θM, φ = φM + φj, with φj denoting the misalignment angle between the Hall bar channel and the [112¯] direction), respectively. RTmax and RLmax represent the amplitudes of the transverse and longitudinal SMR, respectively.

    As shown in Fig. 1(d), the simulated RT curves at 80 K (solid lines) exhibit excellent agreement with the experimental data. Notably, the simulations accurately reproduce the step-like hysteretic features observed in RT. This result validates the selected parameters: Kc1 = −1.25 kJ⋅m−3, Kc2 = 0.48 kJ⋅m−3, Ku1 = 0.60 kJ⋅m−3, Ku2 = 0.30 kJ⋅m−3 and Ms = 96.00 kA⋅m−1. The negative cubic MCA constant Kc1 is consistent with the fact that the 〈111〉 direction serves as the easy magnetization axis in REIG systems.[34] The positive values of Ku1,2 indicate predominant in-plane compressive strain[35] (as detailed in supplementary materials Section 2), which is consistent with the observed IMA of our TmIG film.

    Based on the simulated equilibrium angles (θM, φM), the spatial trajectory of the magnetization is plotted in Fig. 2(a) (see supplementary Fig. S3 for the field dependence of θM and φM). This trajectory clearly reveals four in-plane magnetization reorientation events during the entire field sweep, which correspond to the four jumps observed in the SMR signal. Meanwhile, the azimuthal orientations of the magnetization are separated by discrete steps of 60° and 120°, in good agreement with the 3m rotational symmetry of the system. In our model, the cubic MCA is the sole energy term that exhibits this specific symmetry in the (111) plane. Therefore, this finding strongly suggests that the cubic MCA is the physical origin of the observed anomalous behavior in the SMR signal.

    Figure 2(b) shows the simulated three-dimensional energy distribution of the cubic MCA. In the (111) plane, energy maxima and minima are alternately arranged with intervals of 60°, demonstrating a distinct 3m symmetry. Simultaneously, the energy contours display an antisymmetric configuration relative to the equatorial plane with θM = 90°, where the positions of energy barriers and valleys in the upper and lower hemispheres are distributed in antiphase. This staggered energy landscape imposes strict constraints on the reversal path of the magnetization, preventing it from maintaining a constant azimuthal angle when switching from one pole to the other. This is because the low-energy path initially followed by the magnetization is interrupted by a high-energy barrier upon crossing the equatorial plane. Consequently, driven by the minimization of the total energy, the magnetization must undergo a ΔφM = 60° azimuthal reorientation upon crossing the equatorial plane to align with an adjacent energy valley. Thus, this specific reorientation process appears as a characteristic sharp jump feature in the SMR measurement. The red arrow in Fig. 2(b) schematically illustrates the trajectory of the magnetization during the ascending field sweep. It can be seen that the trajectory tends to follow the energy valleys of the cubic MCA, where the energy is minimized, indicating that the cubic anisotropy plays a dominant role in determining the in-plane alignment of the magnetization.

    Theoretically, if the system maintains perfect in-plane 3m rotational symmetry, the magnetization would be confined to switching between two adjacent inter-hemispheric energy valleys during the field sweep. Consequently, the magnetoresistance curves would exhibit only two jumps near zero field (see supplementary Fig. S4). However, when the magnetic field applied in the experiment contains a small in-plane component (in our measurements, the external field was tilted by 2° with respect to the [111] direction), it breaks this ideal 3m rotational symmetry and lifts the degeneracy of the energy valleys, resulting in secondary switching in the SMR curves.

    To reproduce this physical picture in our simulations, we introduced a 2° tilt of the external magnetic field relative to the [111] axis and a 2° azimuthal deviation from the [112¯] axis. We calculated the normalized total energy distribution as a function of the azimuthal angle (φM) at each field step. As illustrated in Fig. 2(c), this polar plot intuitively visualizes the evolution of the total energy of TmIG at different azimuthal angles throughout the magnetic field sweep. From the polar plot, six blue and red energy branches arising from the cubic MCA are clearly distinguishable, corresponding to the 〈111〉 easy axes and 〈001〉 hard axes, respectively. However, it can be clearly observed that the magnetic field component along the x axis (i.e. [112¯]) breaks the rotational symmetry, yielding energy valleys and barriers at φM = 0° and 180° that are significantly different from those in other directions. During the ascending field sweep, the trajectory of the magnetization orientation (θM, φM) in the polar energy landscape proceeds slowly from the periphery (θM = 180°) toward the center (θM = 0°) because the magnetization tends to remain in-plane due to the strong magnetoelastic and shape anisotropy. Driven by energy minimization, the magnetization initially tracks the energy valley along the φM = 180° direction. However, as the magnetization crosses the equatorial plane into the opposite hemisphere, the energy landscape is inverted, leading to an abrupt ΔφM = 60° jump that switches the magnetization into the adjacent energy valley at φM = 120°. Subsequently, driven by the IP projection of the external field, the magnetization rotates slightly but remains confined within the energy valley at φM = 120° because the finite field projection is not strong enough to overcome the energy barrier at φM = 60°. As the external field is further increased, the IP projection of the magnetic field further breaks the 3m rotational symmetry within the (111) plane, while the OOP projection pulls the magnetization into a canted state. Eventually, the IP component of the external field induces a secondary spin reorientation of ΔφM ≈ 120° into the energy valley at φM = 0°, while θM still changes slowly because the strong easy-plane anisotropy prevents the magnetization from aligning with the OOP direction. This evolution mechanism provides a robust explanation for the sharp-jump signature observed in the field dependence of the SMR.

    Moreover, the magnitude of the SMR is determined by the relative angle between the magnetization M and the nonequilibrium spin accumulation σ (which is always perpendicular to the current density j). For the same magnetization reversal, different SMR responses can be obtained by varying the current direction. Thus, we calculated the SMR curves for different current angles φj. Notably, as shown in Fig. 3, the curves for the configuration in which the current is not parallel to the [112¯] axis (φj = 0°) show the typical bell-shaped profile. This smooth resistance variation signifies a coherent rotation of the magnetization from the in-plane to the out-of-plane direction as the Zeeman energy gradually overcomes the strong easy-plane anisotropy. (The result for a current not parallel to the [112¯] direction is shown in supplementary Fig. S5.)

    To further validate the above physical picture, we performed transport measurements over the temperature range from 3 K to 100 K. As shown in Figs. 4(a) and 4(b), both the transverse and longitudinal SMR exhibit hysteretic resistance jumps with opposite jumping directions, and the critical field for the jumps gradually increases as the temperature decreases. The corresponding simulation results are plotted as solid lines in Fig. 4. Notably, the simulations accurately reproduce the temperature-dependent evolution of both the transverse and longitudinal SMR signals, confirming the validity of our model. As illustrated in Fig. 4(c), the cubic MCA constants (Kc1,2) adopted in the simulations exhibit a gradual increase with decreasing temperature. This behavior is fully consistent with the single-ion model.[36] According to this model, the magnetic anisotropy energy in REIG arises from the combined effects of the crystal and exchange fields on the energy levels of the individual magnetic ions. The Tm3+ ions possess unquenched orbital angular momentum, which leads to significant splitting of their energy levels in the crystal field. As thermal fluctuations decrease at low temperatures, the Tm3+ ions predominantly occupy their ground states, which are highly anisotropic due to crystal-field interactions. This population effect directly results in a rapid enhancement of the cubic MCA constants. The pronounced increase in the uniaxial anisotropy constants Ku1,2 with decreasing temperature is primarily attributed to magnetoelastic coupling induced by thermal stress. Magnetoelastic anisotropy is essentially a change in the MCA induced by stress. Thus, it shares the same temperature dependence as the MCA on the one hand, while increasing with increasing stress on the other hand. Since the TmIG film and the GGG substrate possess different thermal expansion coefficients,[23] the thermal stress increases with decreasing temperature. These effects collectively lead to a substantial increase in the easy-plane magnetoelastic anisotropy energy and a corresponding increase in the saturation field.

    As shown in Fig. 4(d), both the saturation field and the critical fields of spin reorientation increase with decreasing temperature. The correlated evolution of these fields signifies that the topology of the cubic MCA energy landscape remains invariant across the entire temperature range. This implies that the geometric symmetry of the energy valleys and barriers is preserved despite the enhanced anisotropy, resulting in a proportional scaling of the external fields required for reorientation and saturation.

    It is also worth noting that our model elucidates the crystallographic selectivity of this reorientation mechanism: it stems from the broken symmetry of the cubic MCA inherent to (111)-oriented films. Consequently, this mechanism is absent in films epitaxially grown on (110) or (100) substrates,[37] which lack the required energy landscape topology. Finally, we suggest that the analytical framework established herein extends beyond (111)-oriented cubic systems[38,39] and is applicable to rhombohedral or hexagonal systems possessing analogous energy landscapes.[40]

4.   Conclusion
  • In summary, we report an anomalous sharp-jump feature in SMR emerging in (111)-oriented Pt/TmIG heterostructures. By using a three-dimensional Stoner–Wohlfarth model, we successfully determine the complex spin reorientation processes underlying these anomalous SMR signals. Our analysis elucidates how the unique energy landscape of cubic MCA governs the magnetization reversal pathways. Furthermore, we reveal a multiple spin reorientation mechanism driven by the spontaneous mirror-symmetry breaking of cubic MCA, combined with the extrinsic in-plane rotational symmetry breaking induced by the external field. These findings not only demonstrate the significant potential of MCA for manipulating spin states in rare-earth iron garnet systems but also pave the way for the development of novel spin logic and multistate memory devices based on MCA engineering.

Figure (4)  Reference (40)

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return